Shrapnel shell manufacture
The Project Gutenberg eBook of Shrapnel shell manufacture This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Shrapnel shell manufacture A comprehensive treatise on the forging, machining, and heat-treatment of shells, and the manufacture of cartridge cases and fuses for shrapnel used in field and mountain artillery, giving complete direction for tool equipment and methods of setting up machines, together with government specifications for this class of munitions Author: Douglas T. Hamilton Release date: March 15, 2026 [eBook #78213] Language: English Original publication: New York: The Industrial Press, 1915 Other information and formats: www.gutenberg.org/ebooks/78213 Credits: deaurider and the Online Distributed Proofreading Team at https://www.pgdp.net (This
The Project Gutenberg eBook of Shrapnel shell manufacture
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: Shrapnel shell manufacture
A comprehensive treatise on the forging, machining, and heat-treatment of shells, and the manufacture of cartridge cases and fuses for shrapnel used in field and mountain artillery, giving complete direction for tool equipment and methods of setting up machines, together with government specifications for this class of munitions
Author: Douglas T. Hamilton
Release date: March 15, 2026 [eBook #78213]
Language: English
Original publication: New York: The Industrial Press, 1915
Other information and formats: www.gutenberg.org/ebooks/78213
Credits: deaurider and the Online Distributed Proofreading Team at https://www.pgdp.net (This file was produced from images generously made available by The Internet Archive)
*** START OF THE PROJECT GUTENBERG EBOOK SHRAPNEL SHELL MANUFACTURE ***
[Illustration]
SHRAPNEL SHELL
MANUFACTURE
A COMPREHENSIVE TREATISE ON THE FORGING,
MACHINING, AND HEAT-TREATMENT OF SHELLS,
AND THE MANUFACTURE OF CARTRIDGE CASES
AND FUSES FOR SHRAPNEL USED IN FIELD
AND MOUNTAIN ARTILLERY, GIVING COMPLETE
DIRECTION FOR TOOL EQUIPMENT AND METHODS
OF SETTING UP MACHINES, TOGETHER WITH
GOVERNMENT SPECIFICATIONS FOR THIS CLASS
OF MUNITIONS
By DOUGLAS T. HAMILTON
ASSOCIATE EDITOR OF MACHINERY
AUTHOR OF “ADVANCED GRINDING PRACTICE,”
“AUTOMATIC SCREW MACHINE PRACTICE,”
“MACHINE FORGING,” ETC.
_FIRST EDITION_
NEW YORK
THE INDUSTRIAL PRESS
1915
COPYRIGHT, 1915
BY
THE INDUSTRIAL PRESS
NEW YORK
PREFACE
The design of shrapnel and the machining of its component parts
are matters which, at the present time, are of world-wide interest
to manufacturers, engineers, toolmakers, and mechanics in general.
Shrapnel is used in enormous quantities in the great European war,
and American machine tool builders have been called upon to provide
machines and tool equipment of the latest and most efficient design to
meet the demands made upon the manufacturers of shrapnel. Many shops
are running full force, day and night, and are months behind with their
orders. The great importance of shrapnel manufacture, at the present
time, is, therefore, unquestioned.
A small percentage of shrapnel shells are now made from bar stock, but
most shrapnel bodies are made from forgings, formed hollow in hydraulic
presses or in forging machines. The forging processes, which are of
extraordinary interest, especially to those who know something of the
difficulties attending them, are, however, not finishing processes.
Whether made from the bar or forged hollow, all shrapnel shells must be
very accurately finished by machining.
This book has been brought out to meet the demands for a treatise
dealing comprehensively with the construction, forging and machining
operations, and the tool equipment used for making the shell, fuse
parts, and brass cases. In this book are included not only the
unusually complete articles on shrapnel manufacture contained in the
April, 1915, number of MACHINERY, of which 5000 extra copies were
printed and 5000 additional reprints made, all of which have been sold,
but it also includes all other material that has been published at
various times in MACHINERY relating to shrapnel manufacture, together
with a great deal of material obtained by the Editors especially for
this book; and, in addition to this, it contains abstracts of the
official specifications, together with line-engravings of the details
of Russian, British, and American shrapnel shell bodies, fuses, and
cartridge cases. Hence, it is believed that the book will prove
the most valuable addition to the literature on the manufacture of
munitions that has been made since the beginning of the great war.
D. T. H.
NEW YORK, _October, 1915_.
CONTENTS
CHAPTER I.
Shrapnel Shells 1-19
CHAPTER II.
Forging Shrapnel Shells 20-39
CHAPTER III.
Machining and Heat-treatment of Shrapnel Shells 40-74
CHAPTER IV.
Machines and Tools for Shrapnel Manufacture 75-142
CHAPTER V.
Making Fuse Parts 143-171
CHAPTER VI.
Making Shrapnel Cartridge Cases 172-193
CHAPTER VII.
Specifications for the Manufacture and Inspection of the
Russian 3-inch Shrapnel Shell 194-212
CHAPTER VIII.
Specifications for the Manufacture and Inspection of the
Combination Fuse for Russian 3-inch Shrapnel Shells 213-230
CHAPTER IX.
Specifications for the Manufacture and Inspection of
Russian 3-inch Shrapnel and High-explosive Cartridge Cases 231-250
CHAPTER X.
Specifications for British 18-pounder Quick-firing
Shrapnel Shell 251-259
CHAPTER XI.
Specifications for British Combination Time and Percussion
Fuses 260-275
CHAPTER XII.
Specifications for British 18-pounder Quick-firing
Cartridge Case and Primer 276-285
CHAPTER XIII.
Specifications for American Shrapnel Shells 286-292
INDEX 293-296
CHAPTER I
SHRAPNEL SHELLS
In naval, coast defense and artillery operations, several types of
explosive shells are used; the chief ones are: the armor-piercing
shell, made to pierce armor-plate before exploding; shells exploded
by means of a timing fuse; shells exploded by either a timing or
percussion fuse; and shells exploded by percussion only. Each different
shell has some definite function to fulfill, and is designed for
that purpose. For field or artillery operations, the shrapnel and
lyddite are the two principal types used. Of these, shrapnel is the
most prominent, because of its destructive power and its interesting
mechanical construction.
=Early Development of Shrapnel.=--The shrapnel shell was invented
in 1784 by Lieut. Henry Shrapnel, and was adopted by the British
Government in 1808. As is shown at _A_ in Fig. 2, the first shell was
spherical in shape, and the powder or explosive charge was mixed with
the bullets. Although this type of shell was an improvement over the
grape and canister previously used, its action was not altogether
satisfactory, as the shell, on bursting, projected the bullets in all
directions and there was also a liability of premature explosion. In
order to overcome the defects mentioned, Col. Boxer separated the
bullets from the bursting charge by a sheet-iron diaphragm, as shown at
_B_ in Fig. 2. This shell was called a diaphragm shell to differentiate
it from the first shell of this type.
In the shell made by Col. Boxer, the lead bullets were hardened by the
addition of antimony, and as the bursting charge was small, the shell
was weakened by cutting four grooves extending from the fuse hole to
the opposite side of the shell. Shells of spherical shape were first
fired out of plain-bored guns, and upon the advent of the rifled gun
it was necessary to add a circular base, which was made of wood and
covered with sheet iron or steel to take the rifling grooves. The first
shrapnel shells were made of cast iron, but a later development was to
use steel and elongate the body, reducing it in diameter. The diameter
of the bullets was also reduced so that a greater number could be
contained in a slightly smaller space. The improved shrapnel was also
capable of being more accurately directed.
=Shrapnel Shells of Present-day Design.=--Shrapnel shells, as used
at the present time by the different governments, vary slightly in
construction and general contour as well as in the constituents
entering into their different members. As shown in Fig. 1, a completed
shrapnel comprises a brass case carrying a detonating primer and the
explosive charge for propelling the projectile out of the bore of
the gun. The projectile itself comprises a forged shell that carries
the lead bullets and bursting charge. Screwed into the front end is
the combination timing and percussion fuse which can be set so as to
explode the shell at any desired point, and from which the flame for
exploding the bursting charge is conveyed through a powder timing train
and a tube filled with powder pellets down through the diaphragm to the
powder pocket.
Of these members of a shrapnel, the shell and timing fuse present the
most interesting features from a mechanical standpoint. The shell used
by most governments is made from a forging, machined to the desired
dimensions in hand and semi-automatic turret lathes as well as in
ordinary engine lathes. The fuse is an extremely accurate piece of
mechanism, and is largely produced from screw machine parts, some of
which, however, are forged previous to machining. The brass cartridge
case--the next member of importance--is drawn from a brass blank by
successive operations in drawing presses, and is indented and headed.
Following this, several machining operations are performed on the head
and primer pocket.
[Illustration: Fig. 1. Types of Shrapnel Shells used by the American,
Russian, German, French, and British Governments]
=Types of Shrapnel Shells.=--Shrapnel shells are made in two distinct
types, one of which is known as the common shell, and the other as
the high-explosive. The common shell is a base-charged shrapnel,
fitted with a combination fuse, whereas the high-explosive shell is
fitted with a combination fuse and, in addition, with a high-explosive
head, the head also bursting and flying into atoms upon impact. The
high-explosive shell is not ruptured upon the explosion of the bursting
charge in the base, but the head is forced out and the bullets are
shot out of the case with an increased velocity. In the meantime,
the head continues in its flight and detonates on impact. This type
of shell is not used as extensively as the common shrapnel, and,
therefore, the common shrapnel shell alone will be taken up in the
following.
[Illustration: Fig. 2. Original Shell designed by Lieut. Henry Shrapnel
and Col. Boxer’s Improvement]
=The Explosive Charge.=--Reference to Fig. 1 will show that as far
as the construction of the shrapnel shell and case is concerned,
there is very little difference in those employed by the various
governments. Starting with the cases, it will be seen that these are
almost identical, except for length and the arrangement of the head for
carrying the detonating primer. There is a marked similarity in this
respect between the Russian, the British, and the German, and between
the American and the French. The form of the explosive charge held in
the brass case differs in almost every instance, but without exception
smokeless powder in some form or other is used. In the American shell,
nitrocellulose powder composed of multi-perforated cylindrical grains
each 0.35 inch long and 0.195 inch in diameter are used. In the Russian
case, smokeless powder of crystalline structure is used. In the German,
smokeless (nitrocellulose) powder in long sticks and arranged in
bundles is held in the case. The French use stick smokeless powder
¹⁄₂ millimeter (0.0195 inch) thick by 12.69 millimeters (¹⁄₂ inch)
wide. Two lengths or rows of this powder are arranged in the case.
The British use a smokeless powder of crystalline structure somewhat
similar to the Russian, but in some cases cordite has also been used,
although of late this type of powder has not been quite as commonly
employed.
The detonating agent or primer held in the head of the case varies in
almost every type of shrapnel. Practically all primers are provided
with “safety heads,” so that the shrapnel can be handled without danger
of premature explosion. The object, of course, of the detonating agent
or primer is to detonate or cause the sudden explosion of the explosive
charge in the shell for propelling the shrapnel out of the field gun.
=The Shrapnel Shell.=--The shell itself, as previously mentioned,
is made either from a forging or from bar stock. Forgings, however,
are used to a greater extent than bar stock, because the forged
shell is more homogeneous in its structure than the bar-stock shell,
and piping--a serious objection in the bar-stock shell--is entirely
eliminated. The shells used by the British, Russian, and German
governments are made almost exclusively from forgings, whereas those
used by the French and American governments are made both from forgings
and bar stock. When the French shell is made from bar stock, an
auxiliary base is screwed into it to eliminate any danger of piping.
Near the base of all shells is a groove in which a bronze or copper
band is hydraulically shrunk. This is afterward machined to the desired
shape and takes the rifling grooves in the gun so as to rotate the
shell when it is expelled. The body of the shell itself is slightly
smaller than the bore in the gun, and the rifling band, which is
larger and which is compressed into the rifling grooves, rotates the
projectile, thus keeping it in a straight line laterally during flight.
The bursting charge, which in practically all cases is common black
powder, is carried in the base of the shell and is usually enclosed
in a tin cup. Located above this is the diaphragm which is used for
carrying the lead bullets out of the shell when the bursting charge
explodes and distributes them in a fan shape. In most shells, upon
exploding, the nose blows out, stripping the threads that hold the
members together. It will, therefore, be seen that, in the explosion,
the entire fuse, fuse base, tube, diaphragm and bullets are all
ejected, the shell itself acting as a secondary cannon in the air.
The number of lead bullets carried in the 3-inch shrapnel shells ranges
from 210 to 360. In all cases, the lead bullets are about ¹⁄₂ inch in
diameter, weigh approximately 167 grains, and are kept from moving in
the shell by resin or other smoke-producing matrix. The matrix put
in with the lead bullets, in addition to keeping them from rattling,
is also used as a “tracer.” It is of importance in firing shrapnel
that the position of the explosion be plainly seen. With large shells
this is not difficult, but with shrapnel for field guns at long range
certain conditions of the atmosphere make it difficult to see when
the shell actually bursts. Various mixtures are used to overcome this
difficulty. In some cases, fine-grained black powder is compressed in
with the bullets in order to give the desired effect. In the German
shrapnel, a mixture of red amorphous phosphorus and fine-grained
powder which produces a dense white cloud of smoke is used, and in the
Russian, a mixture of magnesium antimony sulphide is used. The range of
a 3-inch shrapnel shell is about 6500 yards, and the muzzle velocity
of the quick-firing field gun ranges from 1700 on the American to 1930
feet per second on the Russian field gun. The duration of flight ranges
from 21 to 25 seconds.
=Development of Timing and Percussion Fuses.=--The first fuses used
in field ammunition were short iron or copper tubes filled with a
slow-burning composition. These were screwed into a fuse hole provided
in the shell, but there was no means for regulating the time of
burning. Later--about the end of the seventeenth century--the fuse
case was made of paper or wood so that by drilling a hole through into
the composition the fuse could be made to burn for approximately the
desired length of time before exploding the shell, or the fuse could be
cut to the correct length to accomplish the same purpose.
For a considerable time all attempts to produce a percussion fuse were
unsuccessful. Upon the discovery of fulminate of mercury in 1799,
the chief requirement of a percussion fuse was obtained. About fifty
years elapsed, however, before a satisfactory fuse was made. The
first percussion fuse was known as the Pettman fuse, and comprised a
roughened ball covered with detonating composition that was released
upon the discharge of the gun. When the shell hit the desired object,
the ball struck against the inner walls of the fuse, exploded the
composition and powder charge, thus bursting the shell. There are at
the present time three principal types of fuses in use: First, those
depending on gas pressure in the gun setting the pellet of the fuse
free--this is a base fuse; second, those relying on the shock of
discharge or the rotation of the shell to set the pellet free--used in
nose and base fuses; third, those depending on impact.
In shrapnel shells advantage is taken of two types of fuses, one of
which is the combination timing and percussion fuse used on common
shrapnel, and the other the combination timing and percussion fuse of
the high-explosive type used on high-explosive shrapnel. These types of
fuses are again sub-divided, but only in the manner of construction.
The most common fuse is that known as the combination timing and
percussion fuse of the double-banked type. This is used in practically
all shrapnel fuses except the French. The advantage of the double ring
of composition shown at _A_ and _B_ in Fig. 3 is to give a greater
length of composition and more accurate burning. Triple-banked and
quadruple-banked fuses on the same principle have been designed, but at
the present time have not been introduced.
=Operation of Combination Timing and Percussion Fuses.=--The manner
in which the combination timing and percussion fuse is regulated to
discharge the bursting charge in the shrapnel shell is interesting and
involves extremely difficult mathematical calculations. Before going
into the method of setting the fuse, it would probably be advisable
to describe briefly just how the fuse operates. As an example of the
double-banked fuse, Fig. 3 shows that adopted by the United States
government. The following description applies to this type of fuse.
[Illustration: Fig. 3. American Type of Combination Timing and
Percussion Fuse used on Shrapnel Shells]
Assume, first, that the timing ring is set at zero. The propelling
force given to the shrapnel shell in leaving the bore of the gun is
such as to sever the wire _C_ from plunger _G_. Plunger _G_ carries a
concussion primer which is discharged by hitting firing pin _D_. The
flame passes out through vent _E_, igniting the powder pellet _F_ and
the upper end of train _A_, and then through the vent _H_. From here,
the flame is transmitted to the lower timing ring _B_ through vent _I_
and the magazine _J_, and from there through the tube to the bursting
charge in the base of the shrapnel shell.
Assume any other setting, say 12 seconds. The vent _H_ is now changed
in position with respect to vent _F_ leading to the upper timing
train, and the vent _I_ leading to the powder magazine _J_ is also
changed. The flame, therefore, now passes through vent _E_ and burns
along the upper time train _A_ in a counterclockwise direction until
the vent _H_ is reached. It then passes down to the beginning of the
lower timing train and burns back in a clockwise direction to the
position of vent _I_, from which it is transmitted by the pellet of
compressed powder in this vent to the powder magazine _J_. It should be
understood that the annular grooves in the lower face of each timing
train do not form complete circles, a solid portion being left between
the grooves in the ends of each. This solid portion is used to obtain
a setting at which the fuse cannot be exploded and is known as the
“safety point.” As shown in Fig. 6, it is marked _S_ on the adjustable
timing ring.
[Illustration: Fig. 4. Russian Type of Combination Timing and
Percussion Fuse used on Shrapnel Shells]
The timing fuse shown in Fig. 3 is of the combination timing and
percussion type, and if the wire _C_ fails to release percussion
plunger _G_, the shell is exploded by means of a percussion fuse
which comes into use when the shell strikes. The percussive mechanism
consists of a primer _K_ held in an inverted position in the center
of the fuse body by a cup located beneath the percussive primer.
Percussion plunger _L_ works in a recess in the base of the fuse body
and is kept at the bottom of the recess away from contact with the
primer by a light spring in plunger _M_. The firing pin _N_ is mounted
on a fulcrumed pin, and is normally kept in the vertical position by
means of two side spring plungers. When the shell strikes, the impact
causes the plunger to snap up against the primer after compressing the
spring in pin _M_. This causes the firing of the primer _K_ and the
explosive charge passes out through a hole in the percussion plunger
chamber, not shown, to the magazine _J_ and from there down to the
powder in the base of the shell
=Russian Fuse.=--The Russian fuse shown in Fig. 4 differs only in a few
minor details from the American fuse, the chief difference being in
the arrangement of the percussive mechanisms. The percussive plunger
for the timing arrangement is kept up from the firing pin by means of
a spring bushing _E_ surrounding the body of the plunger. This bushing
is expanded by the plunger which is forced through it due to the force
of the shrapnel in leaving the bore of the gun. The spring _B_ in the
head of the fuse assists the plunger in expanding bushing _E_ and in
dropping down onto the firing pin _C_. The flame from the exploded
primer then travels down to the powder in the shell in practically the
same way that it does in the American fuse, except that the magazine
chamber is located at _D_ and explodes through the impact fuse chamber.
The percussive arrangement for setting the shell off by impact is
slightly different from that in the American fuse, in that the primer
and firing pin are held apart by means of springs, the inertia of which
is overcome when the shell strikes an object.
=French Fuse.=--With the exception of a few minor details, the timing
fuses used in American, Russian, British, German, Japanese, etc.,
shrapnel shells are the same. The French timing fuse, however, as shown
by the diagram Fig. 5, operates on an entirely different principle. In
this fuse, the firing for the timing train is contained in a sealed
tube of pure tin and is wound spirally around the head of the fuse.
Inside of the head is the ignition arrangement. To set the timing part
of this fuse, it is placed in a fuse-setting machine attached to the
field gun and, by forcing down a handle on this device, a piercing
point is thrust through the outer cap of the fuse, penetrating to the
interior space of the head as shown at _A_. Upon the discharge of
the shell from the gun, the gas pressure forces firing pin _B_ back,
hitting the percussive primer _C_. This causes a flame which passes out
through the opening previously punched at _A_ and ignites the “rope”
powder fuse which is wound around the head of the fuse body. This type
of fuse is also provided with a fuse which sets off the shell by impact
should the timing fuse fail to work. The head of the fuse is covered
with a cap with holes for the piercing point, and the whole cap can
be shifted around for a short distance and set by the corrector scale
marked on the body, as shown in Fig. 1. A projection on the cap engages
a recess in the fuse-setting machine and provides for this movement.
[Illustration: Fig. 5. French Type of Combination Timing and Percussion
Fuse]
=Firing of Shrapnel.=--The accuracy with which a shrapnel can be
exploded in the air at any desired point is remarkable, considering
the number of variable quantities that enter into the construction of
the timing fuse and powder train, etc. The calculations necessary for
finding the correct setting on the timing ring involve, however, the
use of higher mathematics and are consequently not within the scope of
this treatise.
In Fig. 6, the timing ring used on the American fuse is shown. Here
it will be seen that the ring is provided with twenty-one graduations
corresponding to twenty-one seconds in the duration of flight of the
projectile. It will also be noticed that the spacing of the graduations
differs. The reason for this is found in the relation of the vents,
the positions of the lower timing train, the trajectory of the flying
missile, and the decrease of velocity.
[Illustration: Fig. 6. Diagram showing how Timing Ring on the American
Combination Timing and Percussion Fuse is laid out]
Diagram Fig. 7 shows in an interesting manner just how a shrapnel is
fired. The range is approximately obtained by panoramic sights or
other means, and a test shell fired, the point of explosion noted, and
the necessary corrections made. A table which has been worked out for
different distances is then used. In Fig. 7 the diagram shown pertains
to the American quick-firing field gun having a muzzle velocity of 1700
feet per second and the American shrapnel of 3-inch size. It will be
noted that at 2000 yards the terminal velocity of the shrapnel is 1038
feet per second and the time of flight for the projectile 4.75 seconds.
In other words, the timing train to explode the shrapnel at this point
would be set at _A_ in Fig. 6. The range of a 3-inch American shrapnel
is 6500 yards and at this point the terminal velocity is approximately
724 feet per second, the time of flight 21.92 seconds. The shrapnel,
when exploded, shoots out the bullets at an increased velocity or from
250 to 300 feet per second, covering an area of about 250 by 30 yards,
half the bullets falling on the first 50 yards of the beaten zone.
[Illustration: Fig. 7. Diagram Illustrating Path of a Shrapnel and the
Time of Explosion at Various Distances]
In manufacturing shrapnel shells, a test shell is taken from every 120
shells, which is actually fired out of a quick-firing gun into a bank
of sand. If the contour of the shell in the neighborhood of the powder
pocket is expanded during this test, the shell is discarded because of
the liability of tearing out the rifling grooves in the gun
=Propellants and Explosives used in Shrapnel and High-explosive
Shells.=--As has been previously explained, a shrapnel shell contains
three principal parts, _viz._, the projectile that carries the
destructive charge of lead bullets, the fuse that carries a detonating
arrangement for exploding the charge in the base of the projectile,
and the cartridge case that carries the powder charge used in
propelling the projectile out of the bore of the gun. A high-explosive
shell also comprises three principal parts, but the projectile,
instead of carrying a charge of bullets and black powder, is filled
with a high-explosive material, which, when detonated, bursts the body
of the projectile into small pieces that are thrown off with great
velocity and destructive effect. Shrapnel is used against troops in
the open field, whereas high-explosive shells, which may be either
of the ordinary or of the armor-piercing type, are used against
fortifications, etc
=Classification of Explosives.=--The explosives used in shrapnel and
high-explosive shells may be divided into three general classes: 1.
Progressive or propelling explosives--known as “low” explosives. 2.
Detonating or disruptive explosives--known as “high” explosives. 3.
Detonators--known as “fulminates.” The first of these includes black
gun powder, smokeless powder, and black blasting powder. The second,
dynamite, nitroglycerine, gun cotton, etc. The third includes chiefly
fulminates and chlorates. In all classes of explosives, the effect
of the explosion is dependent upon the quantity of gas and the heat
developed per unit of weight and volume of the explosive, the rapidity
of the reaction, and the character of the confinement, if any, of the
explosive charge.
_Low Explosives._--For certain explosives, such as smokeless powder,
the explosive action does not differ in principle from the burning
of a piece of wood or other combustible material. The combustion is
very rapid, but is a surface action, progressing from layer to layer
until the entire grain is consumed. Such materials are known as “low”
explosives, although the power developed through the combustion of
a unit weight may be very great. The progressive emission of gas
from a low explosive, such as burning gun powder, produces a pushing
effect upon a projectile without unduly straining the gun, whereas
the sudden conversion of an equal weight of a high explosive, such
as nitroglycerine, into gas, would develop such high pressures as to
rupture the gun.
_High Explosives._--In high explosives, such as nitroglycerine, gun
cotton, picric acid, etc., the progress of the explosive reaction
is not by burning from layer to layer, but, instead, consists of an
initial breaking up of the molecules, giving rise to an explosive wave,
which is transmitted with great velocity in all directions throughout
the mass, and causes it to be converted almost instantly into a gas.
The velocity of this explosive wave has been determined, for some
materials, to be more than 20,000 feet, or approximately four miles,
per second.
_Detonators or Fulminates._--The action of fulminates is much more
powerful than either the low or high explosives described. They can
be readily detonated by slight shock or by the application of heat,
and are used in primers, for setting off the propelling charge in a
cartridge case, and in fuses, either of the plain percussion or of
the combination time and percussion types. The most common fulminate
is made by dissolving mercury in strong nitric acid and then pouring
the solution into alcohol. After an apparently violent reaction, a
mass of fine, gray crystals of fulminate of mercury is produced. The
crystalline powder thus produced is washed with water to free it from
acid and is then mixed with glass ground to a fine powder. Because of
its extreme sensitiveness to heat produced by the slightest friction,
it is usually kept soaked in water or alcohol until needed
=Manufacture of Black Powder.=--Black powder, because of its “pushing”
effect when exploded, is used extensively as a base charge for shrapnel
shells in expelling the bullets from the projectile. It comprises
three principal elements in about the following proportions: 75
parts of saltpeter, 15 parts of charcoal, and 10 parts of sulphur.
These ingredients must be absolutely free from impurities and, in
manufacturing, great care is taken in refining the saltpeter and
sulphur, and in burning the charcoal, to prevent the introduction
of any foreign substances. After purification, the ingredients are
carefully weighed in the proper proportions and mixed for about 5
minutes in a revolving drum provided with mixing arms. The mixed
charge is now ground for several hours, the charge being moistened
occasionally with distilled water, the resulting mixture being what
is called a “milk cake.” It is then reduced to fine meal in a machine
having Tobin bronze or gun-metal rollers, after which it is compressed
under hydraulic pressure.
The next operation comprises the granulating of the powder, which is
done in a strong Tobin bronze or gun-metal framework carrying two pairs
of toothed and two pairs of plain Tobin bronze or gun-metal rollers.
The “cake” is cut into pieces by these rollers and falls on screens
which sift it into grains of the required size. The grains are then
separated from the dust in a revolving screen, and the high polish or
glaze is produced by putting the powder into drums or glazing barrels,
which revolve constantly for several hours. Graphite is generally used
to provide the glazing effect. The powder is now dried in a stove
heated by steam pipes, and is spread upon canvas trays placed on shelves
=Manufacture of Smokeless Powder.=--Smokeless powder, which is used
in various forms in cartridge cases, was discovered in 1846 by a
German chemist Schoenbein. The chief ingredient of smokeless powder
is cotton. The portion of cotton used is generally the short fiber.
The first attempts to produce gun cotton were unsatisfactory, and
several very serious explosions occurred. Many of the difficulties in
its manufacture were overcome by an Austrian, von Lenk. Still further
progress was made by a Swedish engineer, Alfred Nobel, and the improved
explosive was patented in 1888 under the name of “ballistite.” One of
the principal smokeless powders is known as “cordite”, this name being
derived from the cord-like form it assumes in manufacture. The first
compositions of cordite were: 58 per cent of nitroglycerine; 37 per
cent of gun cotton; and 5 per cent of mineral jelly. This composition,
after considerable use, was found to have a slight deteriorating effect
on the bore of the gun, and after ten years’ use was modified to the
following proportions: 30 per cent of nitroglycerine; 65 per cent of
gun cotton; and 5 per cent of mineral jelly.
The brand of smokeless powder used most extensively as a propelling
charge in shrapnel or high-explosive shells is known as nitrocellulose,
and, as is common with cordite, the base of this is cotton, as
previously explained. It is manufactured as follows: After bleaching
and purifying, the cotton is run through a picker which opens up the
fibers and breaks up any lumps. It is then thoroughly dried and is
ready for nitration. The most generally used method of nitration is
to put the cotton into a large vessel filled with a mixture of nitric
and sulphuric acids. The sulphuric acid absorbs the water developed
in the process of nitration, which would otherwise too greatly dilute
the nitric acid. After a few minutes’ immersion, the pot is rapidly
rotated by power, and the acid permitted to escape. Following this,
the nitrated cotton is washed for a short time and then removed from
the nitrator or pot and repeatedly washed or boiled to remove all
traces of free acid. As the keeping qualities of the nitrated cotton
are dependent upon the thoroughness with which it is purified, the
specifications for powder for the United States army and navy require
that the nitrocellulose shall be given at least five boilings at this
stage of the manufacture, with a change of water after each boiling,
the total time of boiling being forty hours. Following this preliminary
purification, the nitrocellulose is cut up into shorter lengths, by
being rapidly run between cylinders carrying revolving knives. This
operation--known as “pulping”--is necessary because of the difficulty
experienced in removing the free acid, unless the fibers are cut up
into short lengths.
After pulping, the nitrocellulose is given six more boilings, with a
change of water after each, followed by ten cold water washings. The
material is now known as gun cotton or pyrocellulose. Previous to
adding the solvent, this must be free from water. This is generally
accomplished in a circular wringer, and in addition by compressing
the pyrocellulose into solid blocks. Alcohol is forced through the
compressed mass. Ether is then added to the pyrocellulose already
impregnated with alcohol, the relative proportions being two parts,
by volume, of ether to one part of alcohol. After the ether has been
thoroughly incorporated in a kneading machine, the material is placed
in a hydraulic press and formed into cylindrical blocks about 10 inches
in diameter and 15 inches long. It is then transferred to a finishing
press where it is again forced through dies and comes out in the form
of long strips or rods, which are cut into pieces of the length and
widths required. It is in this finishing process that the various
governments differ in their methods of manufacture. The United States
Government uses a short perforated circular block, whereas the French
use flat sticks about 0.0195 inch thick by ¹⁄₂ inch wide. Two lengths
or rows of these sticks are arranged in the cartridge case. The cut
up pieces are subjected to a drying process which removes nearly all
the solvent and leaves the material in a suitable condition for use.
The drying process is a lengthy one, amounting to as much as four or
five months for powder in large pieces. Upon completion, the powder is
blended and packed in airtight boxes
=Manufacture of High Explosives.=--The explosive charges used in
high-explosive shells are known by various trade names, such as:
emmensite, lyddite, melinite, maximite, nitrobenzole, nitronaphthalene,
shimose, trinitrotoluol, turpenite, etc. The base of such explosives as
emmensite, maximite, lyddite, melinite, and shimose, is picric acid,
which is secured from coal tar, subjected to fractional distillation.
The liquid which comes off when this is raised to a temperature of
150 degrees C. is called “light” oil, and when these light oils
have been again distilled, the next fraction or “middle” oil yields
phenol or carbolic acid. This substance when nitrated gives off
picric acid. Experiments with lyddite shells showed their behavior
to be very erratic, some exploding with great effect, while others
gave disappointing results. This was due to the fact that picric
acid requires a powerful detonator to obtain the highest explosive
effect. The use of such a detonator, however, is dangerous, and
extensive experiments have brought forth a new high explosive known as
trinitrotoluol--generally termed T.N.T. Although the explosive force of
trinitrotoluol is slightly less than that of picric acid, the pressure
of the latter being 135,820 pounds per square inch as against 119,000
pounds for trinitrotoluol, its advantages more than compensate for the
difference.
Trinitrotoluol is obtained by the nitration of toluene, contained in
the crude benzol distilled from coal tar and washed out from coal gas.
The crude benzol contains roughly:
Per cent
Benzine 50
Toluene 36
Xylene 11
Other substances 3
Toluene to be used for the manufacture of trinitrotoluol should be a
clear water-like liquid, free from suspended solid matter, and having a
specific gravity of not less than 0.868, nor more than 0.870, at 15.5
degrees C. Trinitrotoluol when pure has no odor and is a yellowish
crystalline powder which darkens slightly with age. It cannot be
exploded by flame or strong percussion, and a rifle bullet may be
fired through it without any effect. When heated to 180 degrees C., it
ignites and burns with a heavy black smoke; but when detonated by a
fulminate of mercury detonator, it explodes with great violence, giving
off a black smoke. Shells containing this explosive, first used on the
western battle front, were given such names as “coal boxes,” “Jack
Johnsons,” “Black Marias,” etc., by the allies.
The Russians and Austrians use a high explosive known as ammonal in
which 12 to 15 per cent of trinitrotoluol is mixed with an oxidizing
compound, ammonium nitrate, a small amount of aluminum powder, and a
trace of charcoal. This high explosive gives somewhat better results
than plain trinitrotoluol, but has the one disadvantage of easily
collecting moisture, and consequently must be made up in airtight
cartridges. The British are now using an improved compound of this
character, which is so prepared that trouble is not experienced with
the collection of moisture.
CHAPTER II
FORGING SHRAPNEL SHELLS
Within the last few months, many methods have been suggested for making
shrapnel forgings, but a comparatively small number have been put into
use. Practically speaking, no two governments have adopted the same
method. The Russian government uses double-acting horizontal hydraulic
forging presses in which two operations are performed at the same time
on different forgings. For instance, while the punch in one end of
the machine is piercing a heated billet, the ram on the return stroke
performs the hot drawing operation on another shell located at the
opposite end of the machine. In this way a shell is completed at each
cycle of the machine--forward and return stroke. The French government,
up to a short time ago, used steam hammers for this purpose, and
produced shrapnel forgings in practically the same manner as a
drop-forging is made, the punch being carried in the ram of the press
and the die held on the bed. This is rather a slow process and requires
more than one heating to complete the forging. The German government
uses a horizontal hydraulic forging press for piercing the billet and
a steam driven machine for drawing the forging, which receives its
motion from a rack and pinion. This method has the advantage over the
hydraulic press of being more economical in the consumption of power.
The methods followed by different concerns in this country and Canada,
at the present time, differ to a large extent. Some manufacturers are
using a method that dates back as far as 1890, as will be described
later. Others are using a more improved method developed about 1895,
whereas about three concerns are using a still more improved method
developed within the past year
=Caley Method of Making Shrapnel Forgings.=--The first method (known
as the Caley process) of making shrapnel forgings in this country had
its inception about 1890 and was used almost exclusively until 1895.
This comprised a slug-forming and billet-piercing operation followed by
a successive reduction and elongation of the forging through drawing
dies. The order of these operations is shown diagrammatically in Fig.
1. The information given herewith pertains to the making of a forging
for a 3-inch shrapnel shell. As shown at _D_, a billet of steel 3¹⁄₄
inches in diameter and 6¹⁄₂ inches long was cut off from a bar with
a cold saw, and formed into a cone shape under a vertical hydraulic
press having a capacity of 100 tons. The billet was heated in a furnace
to about 1900 degrees F., dropped into the impression in the die and
forced into shape by a hydraulic plunger having a depression in the
lower end which centered the blank. The result of this operation is
shown at _F_.
[Illustration: Fig. 1. Diagram showing Caley Process of making Shrapnel
Forgings in Hydraulic Forging Presses]
[Illustration: Fig. 2. Watson-Stillman Hydraulic Forging Press of the
Vertical Type used for making Shrapnel Forgings]
The next step was to anneal the billet, after which it was pierced as
shown at _C_, and at the same time slightly elongated. This operation
was handled in a hydraulic press of the type shown in Fig. 2. On a 0.70
per cent carbon steel billet the pressure on the punch in the piercing
operation was 20,000 pounds per square inch, and the machine used was
a vertical hydraulic forging press of the type referred to having a
capacity of 100 tons. From the piercing operation the forging was
taken direct without annealing to the horizontal hydraulic draw press,
and, as is shown at _H_, was located on a punch and forced through a
series of drawing dies which gradually reduced the shell to the correct
diameter, 3¹⁄₈ inches, and drew it out to the required length, about
8³⁄₄ inches.
A point worthy of attention is the preparation of the cone-shaped
billet. The smallest end was made slightly smaller than the smallest
reduction die in the series. The reason for this was that if any
drawing were done on the end of the shell the front corner would be
drawn over and deformed, increasing the amount of machining required.
The drawing dies in this case were six in number, as shown at _H_,
and were reduced on a sliding scale of the following proportional
reductions. First, 0.100 inch; second, 0.080 inch; third, 0.060 inch;
fourth, 0.040 inch; fifth, 0.030 inch; and sixth, 0.020 inch. This gave
dies of the following sizes, in inches, starting with the largest in
the series: 3.355, 3.275, 3.215, 3.175, 3.145, and 3.125.
The shape given to the drawing edges of the dies is of prime
importance. The mouth or entering side of the hole was beveled to an
angle of 20 degrees leading to a liberal curve which terminated in
a land ¹⁄₁₆ inch wide. The shape was finished off with a ¹⁄₄-inch
radius. These dies were made from chilled cast iron and were held in
position as shown at _H_, being slipped into a pocket in the frame of
the machine, as shown at _I_. The punches for the coning, piercing and
hot drawing operations were made from special hot punching steel. The
first drawing die in the series lasted the longest because the metal
was hotter at this point than when it was drawn completely through the
dies. As a rule, the last drawing die turned out 100 shells before
being worn or scored. Then it was reground to a larger size and used
again. The drawing punch was lubricated occasionally with graphite.
After drawing, the forging is annealed to obtain the proper physical
qualities. This method of making forgings for a 3-inch shrapnel shell
is capable of producing 400 in ten hours.
[Illustration: Fig. 3. Holinger Process of making Shrapnel Forgings]
=Holinger Method of Making Shrapnel Forgings.=--About 1895 the
following method, known as the Holinger process of making shrapnel
forgings, was devised. Instead of making the billet conical in shape
before piercing, this preliminary operation was dispensed with, and to
facilitate the work, as well as to reduce the friction of the flowing
metal, the arrangement of the piercing punch and die was changed. This
process is shown in Figs. 3 and 4, and was accomplished in a hydraulic
press provided with two cylinders, one located at the bottom and the
other at the top of the press.
The operation was as follows: The die _a_ was held in a movable frame
_b_ and the piston _c_ acted first. The first position after the billet
was dropped into the die is shown at _B_. Here the die _a_ and punch
_d_ remained stationary while the piston _c_ descended, pushing the
billet through the die and over the punch. When the piston reached
the end of its stroke, as shown at _C_, the lower cylinder began to
act and the frame carrying the die was raised. This frame, as shown
at _D_, carried a stripper plate _e_ which removed the pierced billet
from the punch and located it so that it could be picked off with a
pair of tongs. A subsequent operation of hot drawing as shown at _E_,
Fig. 4, was required, which is similar to that described in the first
method. The method just described was used chiefly for 6- and 8-inch
shrapnel and projectile forgings, and at the present time is still used
for 3- and 6-inch shell forgings. It requires much less power and turns
out a better and more concentric forging than the method previously
described. The production on 8-inch shells is about 180 in ten hours,
and 250 on the 3-inch shell.
[Illustration: Fig. 4. Holinger Process of making Shrapnel Forgings]
[Illustration: Fig. 5. Improved Method of making Shrapnel Forgings in
One Heat and One Operation]
=Later Methods of Forging Shrapnel Shells.=--The increased demand for
shrapnel within the last few months has been instrumental in bringing
about a radical improvement in the production of forged shells.
Previously, the aim was to get the internal diameter as close as
possible to the finished size and to do comparatively little machining
on it; in fact, this is still, in a great number of cases, one of the
requirements. While at first glance this would appear to be the logical
way of handling the work, on further investigation it is found that
the forging of the shell to the correct size is much more expensive
than to leave sufficient metal to machine all over. In the first place,
a hydraulic machine of 100 tons capacity costs considerably more in
initial outlay than a turret lathe, and in the second place it is more
expensive to operate. The cheapest method of making a shrapnel forging
is to rough-forge it to approximately the correct shape and then finish
to exact shape and diameter in turret lathes or semi-automatic chucking
machines. This simplifies the forging process and also decreases the
production costs.
One of the later methods of making shrapnel forgings is shown
diagrammatically in Fig. 5. A billet of steel 6¹⁄₂ inches long by 3⁵⁄₁₆
inches in diameter is heated to a temperature of from 1900 to 2100
degrees F., and then dropped into the impression in the die _a_ held in
a special cast-steel die-holder _b_. To do this, die _a_ is drawn out
from beneath the punch, punch guide _c_ removed, and the billet dropped
in. Then the guide is replaced and the die-holder slid in until it
contacts with the stop _d_. The press is now operated, and, as shown at
_B_, advances, piercing the billet and making the metal flow up around
the walls of the punch.
The punch now retreats, carrying the centralizing guide _c_ with
it. The die-holder is now drawn out from under the punch onto a
bracket projecting from the bed of the press. The high-carbon steel,
hardened block _e_ then drops out of the die, as is also the case
with the finished forging. This block _e_, of course, is heated up
to a considerable extent due to the hot metal resting on it so that
several blocks of this kind are provided. In the illustration, as
shown at _C_, centralizing guide _c_ is shown attached to the punch.
In actual operation this is not the case. When the punch rises, guide
_c_ is stripped from it by stripper plate _f_ so that the guide is
gripped with tongs and laid down on the bed of the press until a fresh
heated billet has been placed in the die impression ready for the next
piercing. The punch is made from special hot punching steel and the die
from chilled cast iron. The production of forgings by this method for a
3-inch shrapnel shell is about 600 in ten hours.
[Illustration: Fig. 6. Producing Shrapnel Forgings in a 750-ton
Hydraulic Forging Press]
The amount of metal left for machining by this method varies from
¹⁄₈ to ³⁄₁₆ inch on the internal and external diameters. The forging
after annealing is then machined inside and out on turret lathes,
or semi-automatic chucking machines. The accepted method is to first
machine the internal diameter and then hold the shell on an expanding
arbor and machine it on the external diameter.
[Illustration: Fig. 7. Piercing Billets for Shrapnel Forgings In a
“Wood” 750-ton Hydraulic Forging Press]
=Producing Shrapnel Forgings in Hydraulic Presses.=--In the foregoing
description various principles of making shrapnel forgings were
described. Owing to the large number of forgings lately required,
practically all types of forging presses and power forging machines
have been used. Fig. 6 shows how one manufacturer is solving the
problem. The machine used is an R. D. Wood Co., 750-ton hydraulic
forging press; this performs both the billet piercing and drawing
operations. The forgings turned out on this machine are for the British
18-pound shell, and the billet is 3¹⁄₂ inches in diameter by 4¹⁄₂
inches long. The first operation, piercing the billet, is done by the
punches and dies shown in Fig. 7. The billet is heated in a furnace to
a temperature of 2000 degrees F., and then quickly removed and placed
in the dies. The press is now operated, piercing two billets at the
same time. The pierced billet is 3¹⁄₂ inches in diameter by 7¹⁄₂ inches
long.
A complete batch of pierced billets is first put through, then the
pierced billets are taken to the furnace again and heated to 2000
degrees F. The punches and dies in the center of the illustration Fig.
8 are used for finish-drawing the forging by drawing it out to 3¹⁄₂
inches in diameter by 11 inches long. This method is only temporary
and will be replaced shortly by three R. D. Wood four-post hydraulic
presses. The piercing operation will be handled on one press of 350
tons capacity, and the drawing operations on two presses of 200 tons
capacity.
[Illustration: Fig. 8. Drawing Shrapnel Forgings in a “Wood” 750-ton
Hydraulic Forging Press]
=Making Shrapnel Forgings in Power Forging Machines.=--One of the
latest developments in the art of producing forgings for shrapnel
shells is the adaptation of the power forging machine to this work. As
has been previously mentioned, there are several methods of producing
shrapnel shells, and as it has been conclusively proved that the
forged shell is superior to the shell made from bar stock, it is
only natural that several methods for making the forgings would be
developed. In the forging machine method, a bar slightly larger than
the finished diameter of the forging is cut off, making a billet about
5¹⁄₂ inches long. This billet, for a 3-inch shell, weighs about 9¹⁄₄ to
9¹⁄₂ pounds.
[Illustration: Fig. 9. Examples of Shrapnel Forgings turned out on a
Power Forging Machine]
The billet is heated to a white heat in a furnace, the temperature
being about 2000 degrees F., depending on the carbon content and
other constituents in the steel, and is then placed in the lower
impression of the forging die. The machine used for this size of
forging is a standard upsetting and forging machine provided with a
special crank-shaft. Upon being operated, the lower plunger, which is
larger than the diameter of the powder pocket in the shell, advances
and pierces the billet. The pierced billet is then raised to the next
impression, and the machine again operated. The second punch is longer
than the first and smaller in diameter. The billet is forced up on this
punch, which reduces it in diameter and increases its length. After
the second impression the partially formed shell is then placed in
the third or final die impression, where it is given two blows, being
given one-half turn after the first blow to form it more perfectly. The
operations just enumerated are performed in one heating of the billet,
and the production of a 3-inch shell ranges from 400 to 450 in ten
hours.
The dies for this work are, of course, constructed upon a somewhat
different principle from the ordinary forging die, because in this case
it is necessary to make the metal flow up on the punches. The dies,
therefore, are so constructed that they recede as the punch advances,
which tends to make the metal flow up on the punch. The practicability
of this method is well illustrated by the samples shown in Fig. 9. Here
_D_ is the rough forging just as it comes from the machine, with the
exception that the mouth has been trimmed. _C_ is a section of a shell
made from low-carbon steel about 0.30 per cent carbon; _B_ is a shell
made from 0.50 per cent carbon, 3¹⁄₂ per cent nickel steel. This has
been rough-turned, as the illustration shows. The homogeneity of the
forgings is clearly indicated. _A_ is a forging made from low-carbon
steel, finish-turned.
One of the most interesting points about this method is its cost as
compared with shells made from bar stock. To produce a 3-inch shell
from bar stock requires about 22 pounds of material, and on metal
costing 10 cents per pound, a bar shell--exclusive of machining--costs
$2.20; to produce the same shell on a power forging machine requires
about 9¹⁄₄ to 9¹⁄₂ pounds, and figuring on 10 cents per pound the
cost for the material is only $1--a saving of $1.20 on each shell.
Furthermore, the production of shells from bar stock on automatic
machines is about twelve to fifteen per day. The number of forgings
that can be turned out in the same time is 400 to 450, and the number
that can be machined in this time varies from forty to fifty for two
operations. It is therefore evident that the production of shells by
forging is far superior to the bar method, and the forged shell is more
satisfactory from every standpoint.
[Illustration: Fig. 10. Diagram Illustrating Method of piercing and
drawing Shrapnel Forgings in a Bliss Power Press]
=Forging Shrapnel in a Power Press.=--Another interesting development
in the forging line is shown diagrammatically in Fig. 10. This method
comprises three operations, and is handled in a No. 80¹⁄₂ Bliss press
capable of exerting a pressure of 1200 tons. A billet 3¹⁄₄ inches in
diameter by 3³⁄₄ inches long is heated in a furnace to 1976 degrees
F. and then quickly placed in the die shown at _A_. The press is
operated, and the punch in descending pierces the billet, being guided
by the guide _a_, as shown at _B_, which also acts as a stripper. The
forging retains its heat to a certain extent after this operation, the
temperature being about from 1380 to 1425 degrees F. This is sufficient
to perform the second minor operation which, as shown at _C_ and _D_,
consists in forcing the heated billet into the die-block to reduce the
diameter of the lower end and facilitate the succeeding operation. This
reducing operation is performed with the same type of punch as is used
in the succeeding operation, and the die-block is simply laid on top of
a bolster while the reducing is being done.
The final forming or drawing of the forging is accomplished as shown at
_E_ and _F_, the same type of press, _viz._, a Bliss No. 80¹⁄₂ power
press, being used for this purpose. The pierced billet is now heated
to 1976 degrees F., and is then forced through the three drawing dies
_b_, _c_ and _d_, by the punch _e_. The first die is 3⁵⁄₁₆ inches in
diameter and reduces the forging from 3³⁄₈ inches to this size. The
second is 3⁷⁄₃₂, and the third, or last, 3¹⁄₈ inches in diameter.
The forging, after being forced through the dies, is stripped from
the punch by plates _f_, and as it still retains a temperature of
1475 degrees F.--sufficient for annealing--is thrown down on the
sand to cool off. The billet piercing and drawing dies, shown in the
illustration, were made from 50-point carbon steel, hardened. This gave
fair results, although chilled cast-iron dies would prove even more
satisfactory. The punches were made from several different materials
such as chrome-vanadium, 70-point carbon steel, and unannealed
malleable casting. Of the three materials, the latter gave the most
satisfactory results, in that pitting was reduced to a minimum. Of
course, it was necessary to grind the malleable casting to shape.
=Flow of Hot Metal When Pierced.=--In the manufacture of shrapnel shell
forgings, the first operation is that of piercing, and to accomplish
this satisfactorily, it is necessary to understand the action of a
piercing punch on a semi-plastic billet of steel. There are certain
fundamental laws governing the flow of metals under pressure and a
study of these is of exceptional interest. An attempt has been made
in Fig. 11 to illustrate diagrammatically some of the principles
involved, and in the following discussion it should be understood that
the billet is made from 50-point carbon, 60-point manganese steel, 6¹⁄₂
by 3⁵⁄₁₆ inches in diameter.
At _A_ a round-end tapered punch is shown in contact with the heated
billet, and the lines show the possible flow of the metal, _i.e._, the
material commences to “pack” at the end of the punch. In this case the
walls of the die are straight. At _B_ the billet is being pierced,
and the resultant effect on the flow of the metal is indicated. Here
it will be seen that the pressure increases as the punch descends,
because of the wedging action on the metal and the friction between the
surfaces of the sides of the punch and die. The pressure on the end of
a punch of this shape is about 20,000 pounds per square inch.
[Illustration: Fig. 11. Diagram Illustrating Flow of Hot Metal while
being pierced]
By leaving the sides of the die of the same shape as at _B_, but
making the end of the punch square instead of round and not tapered,
different action is caused. When the flat punch, as shown at _C_, first
contacts with the metal, the pressure required is greater than at _A_,
but as soon as the metal commences to flow as at _D_, the pressure
decreases. For instance, suppose the pressure required at _B_ to pierce
the billet was 100 tons; on the same material at _D_, the required
pressure would be only 70 tons--a decrease of 30 per cent. The metal,
however, does not follow the sides of the punch as closely at _D_ as
at _B_, and this accounts in part for the reduction of power required.
The action of hot flowing metal on the face of a square punch is just
the reverse of what would naturally be expected. Instead of the punch
wearing away at the edge, the center first shows signs of wear as
indicated at _e_. Seams are opened up in a radial direction caused by
the hot metal attacking the softest parts in the face of the punch.
[Illustration: Fig. 12. Shrapnel Shell Head and Diaphragm produced in a
Power Forging Machine]
Again, a different condition exists to that shown at _B_ and _D_,
when both the die and the punch are tapered as shown at _E_. Here the
friction of the extruded metal on the walls of the die and sides of
the punch is excessive, and it is practically impossible to produce
a satisfactorily pierced billet in this manner. From a theoretical
standpoint, the conditions shown at _F_ are ideal. Here the sides of
the punch are straight, the end flat, and the walls of the die taper
or increase in diameter toward the bottom. In this case the friction
of the flowing metal is greatly reduced because of the lessening of
the wedging action. Other considerations, however, make this method
impracticable.
[Illustration: Fig. 13. Diagram Illustrating Method of producing
Shrapnel Shell Heads in a Power Forging Machine without any Waste of
Stock]
A still greater reduction in the pressure necessary to pierce a billet
is shown at _G_. Here a square billet instead of a round one is being
pierced. In the plan view it will be noticed that the friction on the
walls of the die is greatly reduced, and the pressure continues low
until the extruded billet contacts all around with the surface of the
die. The completed product, however, is inferior to that made from a
round billet. From the previous remarks, it will be seen that a punch
and die that would best meet the requirements is one having a rounded
end as at _B_, straight sides as at _D_, and straight walls in the die.
The most satisfactory punch and die for piercing shrapnel forgings when
all the variable conditions are considered would be as shown at _H_.
[Illustration: Fig. 14. Diagram Illustrating Method of making Shrapnel
Shell Diaphragms in a Special Type of Power Forging Machine]
=Forging the Shrapnel Head.=--The shrapnel head shown at _A_ in Fig.
12, that screws into the end of the shell and into which the fuse body
is screwed, is made from a forging of low-carbon steel for the French
shell. One method of producing this, which is of unusual interest,
is shown in Fig. 13. A power-driven forging machine equipped with a
special set of tools is used for this purpose. A bar of steel of the
same diameter as the hole in the finished forging, in this case 1¹⁄₂
inch, is gripped in the dies as shown at _A_, and is upset by means
of a plunger _a_, forming an upset on the end of the bar shown to
the right. The upset bar is now placed in the second impression of
the gripping dies, as shown at _B_. By way of explanation, it should
be stated that the views of the dies shown at _A_, _B_, and _C_ are
sections taken in a horizontal plane at each stage or die impression.
Upon gripping the upset forging in the second impression in the dies,
the plunger _b_ advances and forms an annular groove in the face of the
forging, at the same time increasing its width as shown at _c_.
The forging, still integral with the bar, is now quickly removed and
placed in the last impression of the dies. The diameter of the hole
in these dies is larger than the bar, allowing it to slip back as
the punch advances to punch the hole in the forging. When the punch
moves forward it carries with it the spring-operated sleeve _d_, thus
finishing the forging in one heat. This method of forging is very
satisfactory, producing a homogeneous forging at the rate of 1500 in
ten hours.
=Forging the Steel Diaphragm.=--The steel diaphragm shown at _B_ in
Fig. 12 is made from low-carbon steel in a special type of forging
machine operated similarly to a hot-pressed nut machine. That is to
say, the bar, instead of being fed in from the front, as in a regular
forging machine, is fed in from the side. The manner in which this is
accomplished is shown in Fig. 14. A flat bar of steel 2³⁄₈ inches wide
by ³⁄₈ inch thick, heated to the proper temperature for a distance of
three feet, is fed across the face of the die as at _A_ and located by
stop _b_. Punch _c_ then advances and cuts out a blank of the required
diameter, forcing it into the die, as shown at _B_. The metal is now
confined between the faces of punches _d_ and _c_ and in die _a_, and
is forged to the required shape. The next step is shown at _C_, where
punch _d_ advances and forces the formed forging out of the die. The
production of this diaphragm is in the neighborhood of from 8000 to
10,000 in ten hours.
CHAPTER III
MACHINING AND HEAT-TREATMENT OF SHRAPNEL SHELLS
[Illustration: Fig. 1. Shrapnel Shells in Various Stages of Manufacture]
Shrapnel shells are manufactured either from bar stock or forgings. The
bar-stock method, however, is not considered as satisfactory as forging
because of piping, so that the greater number of shrapnel shells made
at the present time are turned out from forgings. The first step,
therefore, in the making of a shrapnel shell is to cut off a billet of
the required length from a bar of steel of the necessary constituents.
In the making of an 18-pound shrapnel shell, the billet is cut off
from a bar of 46-point carbon, 60-point manganese steel in machines of
different types. One way of doing this, as shown in Fig. 2, is to use a
Newton cutting-off machine having an air clamp for holding the bar in
place while it is being cut off. A Hunter duplex saw, as shown in the
illustration, provided with high-speed steel inserted teeth, performs
the cutting operation. The billet for an 18-pound shrapnel shell is
3¹⁄₂ inches in diameter by 4¹⁄₂ inches long. It is then forged to
shape, as has been previously explained.
Assuming that the forging has been completed, the following is a
complete summary of the machining operations on the shell up to the
point of assembling. In one plant where this work is being done, the
shrapnel shells are put through in lots of 120, each lot being kept
in three boxes, forty shells to a box. Out of every 120, one shell
after heat-treatment is tested for tensile strength. The tensile
strength before heat-treatment must be from 30,000 to 40,000 pounds per
square inch, and from 80,000 to 90,000 pounds per square inch after
heat-treatment. For facilitating transportation, trucks of various
designs are used. One type of truck used for this purpose is shown in
Fig. 3. This is built by the Chapman Double Ball Bearing Co. of Canada,
Ltd., Toronto, Ontario, and has some interesting features, the chief of
which are the ball-bearing swiveling head, ball-bearing wheels, and the
means of releasing or raising the load with the handle in any position.
This feature is valuable in using the truck in a crowded space.
[Illustration: Fig. 2. Cutting off Billets for making Shrapnel Forgings
in a Newton Cutting-off Machine]
=Trimming and Facing the Shell Forging.=--The first machining operation
on the forged shell is to cut off the ragged end, which is generally
from ¹⁄₂ to 1¹⁄₂ inch longer than that required for the finished shell.
This operation is performed in many different ways, but one of the
most common is to place it in a Hurlbut-Rogers cutting-off machine as
shown in Fig. 4. For performing the cutting-off operation, two plain
forged cutting-off tools made from “Sabine” extra high-speed steel are
used. The forging is located in the proper position in the chuck by
a plunger or stop _A_, sliding in a fixture _B_ clamped to the base
of the machine. This plunger locates the shell from the bottom of the
hole or powder pocket and forces the shell into the chuck against the
resistance of an open-wound spring. The stop is then located by a gage
_C_ that forms a member of the fixture and fitting ring _D_ on the
stop. The chuck jaws are now clamped on the work and the cutting off
commences. As soon as the excess stock is cut off, the stop is drawn
back and the pressure of the jaws on the work released; the spring in
the chuck then ejects the forging. The production of an 18-pound shell
from one machine is about 140 in eight hours.
[Illustration: Fig. 3. Truck built by the Chapman Double Ball Bearing
Co. for transferring Shrapnel Shells about the Shop]
The next roughing operation is to face off the bottom or closed end of
the forging, bringing the shell to approximately the correct length.
There are also many ways of performing this operation. One method is to
grip the forging in a chuck, as shown in Fig. 5, in an ordinary lathe
and face off the end with a high-speed steel tool held in an Armstrong
tool-holder. From to ¹⁄₄ to ³⁄₈ inch is faced off from the end.
[Illustration: Fig. 4. Cutting off Excess Length of Shrapnel Forging in
a Hurlbut-Rogers Cutting-off Machine]
[Illustration: Fig. 5. Facing off Closed End of Shell to Length]
=Rough-turning Operations on Shrapnel Forging.=--Practically every type
of engine lathe and turret lathe as well as special machines are used
for turning and boring shrapnel forgings, and in the following chapter
each method will be dealt with separately. Before doing this, however,
a complete summary of the methods of machining employed in a large
plant turning out shrapnel will be described. In this plant, the first
rough-turning operation is handled on a flat turret lathe, as shown in
Fig. 6. For this purpose, the shell forging is held on an expanding
arbor and is driven by a dog fastened to it and driven by the faceplate
of the lathe. A multiple tool turner is first brought into position and
takes a cut of about ¹⁄₈ inch from the diameter for practically the
entire length of the shell. The next tool then faces off the end of the
shell to length.
[Illustration: Fig. 6. First Rough-turning Operation on Shrapnel Shell
in a Flat Turret Lathe]
The shell forging is now ready for cutting the rifling band groove
and producing the waves. This is handled in an ordinary engine lathe
equipped with a special fixture, carrying grooving, waving and
under-cutting tools. The shell forging, as shown in Fig. 7, is held in
a chuck at one end and supported by a revolving center at the other.
One part of the fixture is clamped to the bed of the lathe and the
other to the carriage. The grooving and ribbing is accomplished with
a tool held in holder _A_ at the front of the lathe, whereas the two
under-cutting tools are held in holders _D_ and _E_ at the rear of
the lathe. In operation the carriage of the lathe is moved toward the
chuck, carrying the fixture to which are fastened cams _C_, _F_, and
_G_. Cam _C_ forces in the holder carrying the combination grooving and
ribbing tool, whereas cams _F_ and _G_ force in the holders carrying
the two under-cutting tools, these being presented at an angle to the
work. The required oscillations to the slide carrying the grooving and
ribbing tool are secured through a face-cam _B_ clamped to a “Whiton”
chuck. The face-cam operates against the tension of spring _H_ and
gives the required oscillations to the tool-slide carrying the ribbing
and grooving tool, shown at _A_.
The third machining operation is accomplished in a flat turret lathe,
as illustrated in Fig. 8. This consists in facing the open end of the
shell, boring the powder pocket and facing and boring the diaphragm
seat, and also turning the angular surface on the external nose of the
shell. First, a roughing drill is brought in to rough out the powder
pocket. The turret is then indexed and a tool for turning the angle
of the nose is brought into position. The machining on the nose is
then accomplished by operating the cross-sliding head. Then a roughing
cutter is brought in to rough-bore the powder pocket. The turret is
again indexed and a finishing tool is brought in to finish the powder
pocket and face the diaphragm seat. This finishes the machining
operations on the shell previous to heat-treatment.
[Illustration: Fig. 7. Cutting the Rifling Band Groove with a Special
Grooving and Ribbing Attachment on an Engine Lathe]
[Illustration: Fig. 8. Third Machining Operation on Shrapnel Shell in
a Flat Turret Lathe, consisting in Facing the Open End of the Shell,
Boring the Powder Pocket, Facing and Boring the Diaphragm Seat, and
Turning the Angular Surface on the External Nose of the Shell]
[Illustration: Fig. 9. Heat-treating Shrapnel Shells, using a Hoskins
Electric Barium-chloride Bath Furnace]
[Illustration: Fig. 10. Testing Hardness of Shrapnel Shells with Shore
Scleroscope]
=Heat-treating Shrapnel Shells.=--As was previously stated, the tensile
strength of a forged shrapnel shell after heat-treatment must be from
80,000 to 90,000 pounds per square inch, and in order to obtain the
desired physical qualities, it is necessary that the heat-treating
operations be properly conducted. Several methods of heat-treating
employing different cooling solutions are used in the manufacturing
plants making shrapnel shells. One method, as shown in Fig. 9, is
to heat the shell in a Hoskins electric furnace that contains a
barium-chloride bath, heated to a temperature of about 1480 degrees F.
The shells are left in this furnace for half an hour and are taken out
and dipped in a bath of cottonseed oil heated to a temperature of 113
degrees F. The temperature to which the shell is heated varies with the
different constituents of the steel and practically every different
batch of 120 shells requires a slightly different temperature.
The proper temperature is determined by cutting out a section of a
heat-treated shell and testing it for tensile strength. The next step
is to draw the temper on the open end of the shell. In this operation
a muffle gas furnace heated to a temperature of about 1000 degrees F.,
is used. The temper is drawn for about two-thirds of the length of the
shrapnel shells.
=Testing for Hardness and Tensile Strength.=--One shell from a batch
of 120 is now cut open in the proximity of the powder pocket and the
cut-out section sent to the government inspectors to test it for
tensile strength. Each one of the shells in the batch, in addition, is
tested for hardness by a Shore scleroscope as shown in Fig. 10. Before
testing for hardness, the shell near the band groove is polished so
as to get a true reading, then placed in a fixture, and the hammer of
the scleroscope allowed to drop on it. The reading should be between
40 and 50, indicating an elastic limit of from 80,000 to 90,000 pounds
per square inch. The shell must not be ruptured at the point tested
when the charge in it is exploded or when the charge in the case is set
off. Should the shell upset near the rifling band groove when it is
propelled out of the gun, it would tear out the rifling in the bore of
the gun.
Experience with the scleroscope has disclosed the existence of a
fairly definite relation between the hardness and strength of metal.
In determining the strength of metal, two stages are recognized:
First, the elastic limit, determined by the load required to produce a
permanent set; second, the ultimate strength, determined by the load
required to cause rupture. The hardness indicated by the scleroscope is
intimately related to the elastic limit. The elastic limit increases
more rapidly than the hardness from 43 to 45, this being the minimum
index of the strength value required. As an elongation of 8 per cent in
2 inches is also required, there must necessarily be an upper limit to
the hardness. On the steel used for shrapnel, which is generally about
50-point carbon and 60-point manganese, the maximum hardness should not
be over 60 on the scleroscope.
=Tests relating to Heat-treatment of Shells.=--In the September, 1915,
number of MACHINERY, Mr. J. M. Wilson, who has been actively engaged in
heat-treating shells since the beginning of the war, and who has had
to rely entirely upon his own resources in meeting and overcoming the
troubles which seemed to arise on all sides, relates the results of his
experiments.
[Illustration: Fig. 11. Cross-sectional View of Shrapnel Shell showing
Points A, B, and C where Tests are made, and one of the Tensile Test
Samples]
The British government shell specifications call for a yield point
or elastic limit, after heat-treating, of not less than 36 tons per
square inch, a breaking point or ultimate strength not less than 56
tons per square inch, and an elongation not less than 8 per cent in
⁵⁄₈ inch. Officially there is no maximum specified for either of those
three physical characteristics; but as a matter of fact any unusual
condition which is not in conformity with recognized metallurgical
practice may cause the chief government inspector for the district in
which the manufacturer is located to reject a shipment. Reference has
been made to certain points in the shell which must resist the strains
due to firing. The nature of these strains and condition of the steel
best suited to meet them will be understood from Fig. 11, which shows a
cross-section of the British 18-pound shrapnel shell. When a shell is
fired from a gun, the base _A_ is subjected to a blow, _i.e._, a sudden
increase of pressure which almost instantly attains a maximum of from
12 to 14 tons per square inch, and imparts the initial velocity to the
shell. The shell, being a body at rest, opposes this velocity with its
own inertia, the result being that both compressive and tensile strains
are set up in the shell body. The shell body assumes the conditions of
a column which has a compressive load varying from nothing at the nose
to a maximum at the base. The tensile load is due to the inertia of the
bullets inside the shell. These bullets are subject to an increasing
compressive load from the top down, the resultant strain being a
bursting effort which attains a maximum in the region of the point _B_,
known as the “set-up point.”
When the time required for the fuse to act has elapsed, the powder
charge is exploded, and the contents of the shell are blown forward in
the usual manner. The contents are released either by the stripping of
the thread of the brass socket, or else the walls of the shell yield at
the point _C_, opening the threads sufficiently to free the socket. At
_A_, (the base) the shell must be perfectly sound and free from flaws
such as minute cracks, etc., which may allow the flame from the firing
charge to strike through with disastrous results to the shell and gun.
The metal in the base must not be too hard or it may fracture under
the pressure of the explosion, and it must not be too soft or it may
flatten out and spoil the rifling in the bore. At the point _B_ there
is no maximum requirement so far as tensile strength is concerned, but
any abnormal strength is viewed with suspicion unless it is accompanied
by a generous elongation. At _B_ the metal is particularly liable to
distension while the shell is acquiring velocity, and unless the shell
is strong enough to resist the sudden bursting strain, and the amount
of elongation is sufficient to cushion or absorb this strain at the
instant of firing, the shell is liable to take a permanent set in the
region of point _B_, with results mentioned above. The shell must not
be too hard at the point _C_ as it may burst, thus neutralizing the
real object of a shrapnel shell which is to project the bullets forward
with increased velocity at the predetermined instant, being in fact an
aerial gun arranged to discharge its contents at any desired point of
its flight.
=Uniformity of Steel for Shrapnel.=--Having these requirements firmly
established in his mind, the heat-treating expert is now confronted
with a double problem: How is it possible to give steel the suitable
strength; and having done so, how is it possible to know that the
desired result has been obtained, without actually making test pieces
from each shell. The principal condition upon which successful
heat-treating depends is uniformity of material. Carbon and manganese
are the principal substances which influence the results. The exact
composition of steel specified by the government is not given to
any manufacturers other than steelmakers. It is, however, generally
understood to be a 0.50 per cent carbon, 0.60 per cent manganese steel.
Allowing five points variation in carbon and ten points variation
in manganese, the requirements would be approximately 0.45 to 0.55
per cent carbon and 0.50 to 0.70 per cent manganese. In one carload
of forgings, one firm received shells from 23 different heats or
melts, with carbon varying from 0.60 to 0.47 per cent, and manganese
varying from 0.63 to 0.49 per cent, with all possible combinations
and proportions between these limits. The number of forgings supplied
from each heat varied from one up to 1200 so that the question of
determining the best temperature for each carbon content was indeed
quite impracticable. Many manufacturers at the present moment may be
in a similar position, and the gravity of the situation, both from a
financial and a military point of view, may justify a somewhat detailed
description of the method which was followed in treating shells of such
varying composition.
=Results of Tests.=--It is generally known to manufacturers that the
highest tensile strength of steel is obtained by cooling it rapidly
from a temperature slightly higher than the decalescent point or
critical temperature. The degree of hardness resulting from this
operation can be ascertained quickly, accurately, and repeatedly by
means of the scleroscope. The degree of hardness thus shown is a
reliable indication of the probable strength of the material; that is
to say, after making due allowance for different makes of steel and
varying proportions of the principal constituents, the scleroscope
readings are a reliable indication of the results which may be expected
when a tensile test is made of any given shell. In the opening months
of the shell business, considerable reliance was placed on the accurate
determination of the decalescence point. Forgings of varying analysis
were received; the carbon being from 0.48 to 0.53 per cent, and the
manganese from 0.54 to 0.69 per cent. All steels whose composition was
within those limits showed a decalescence point of between 1390 and
1425 degrees F., and when quenched in water at 50 degrees F. above
the decalescence point, such steels would have a scleroscope hardness
number as high as 85; but when quenched in ordinary fish oil the
hardness was only slightly over 50, the sample being 1 inch square and
¹⁄₈ inch thick. A complete shell quenched in fish oil would show a
scleroscope hardness number at the set-up point of from 38 to 40. Test
pieces from such a shell failed to reach the minimum breaking strength
of 56 tons by the narrow margin of 0.6 ton, and this failure brought
up the question of which was the best quenching medium. A series of
experiments gave the results presented in Table I; all conditions were
equal in each test, and the test pieces were all made from the same
forging.
TABLE I. RESULTS OF TESTS TO DETERMINE THE BEST QUENCHING MEDIUM FOR
SHRAPNEL SHELLS
+-------------+----------------+--------------------+---------------+
| Quenching | Quenching | Temperature of | Scleroscope |
|temperature, | medium | quenching | hardness No. |
| degrees F. | | medium, degrees F. | |
+-------------+----------------+--------------------+---------------+
| 1475 | Fish oil | 90 | 50 to 55 |
| 1475 | Coal oil | 90 | 65 to 70 |
| 1475 | Cottonseed oil | 90 | 70 to 75 |
| 1475 | Engine oil | 90 | 75 to 80 |
| 1475 | Oil of degras | 90 | 77 to 85 |
| 1475 | Water | 90 | 82 to 87 |
+-------------+----------------+--------------------+---------------+
_Machinery_
From the results of the tests presented in Table I, oil of degras,
commercially known as “No 2 soluble quenching oil,” was selected as the
quenching medium and operations were commenced on forgings supplied
from two separate heats. The results were all that could be desired
until forgings were received from a certain heat, which would not
respond to treatment based upon the results of preliminary experiments.
Investigation yielded the results presented in Table II. While
water-treatment of the forgings from “Heat No. 3” gave satisfactory
strengths under test, the liability of shells to crack, owing to
their thin walls contracting more rapidly than the base, was a fatal
objection to this method. Attention should be called to the fact that
while the temperature at which quenching should be done is specified by
the government at 1560 degrees F., manufacturers are not tied down to
this particular temperature. What is required is that the manufacturers
shall so treat the material that it will fulfill the requirements
already stated. If, when fulfilling these requirements, the treatment
should prove detrimental to the shell in other respects, then it must
be changed accordingly.
TABLE II. RESULTS OF TESTS CONDUCTED TO SECURE GENERAL DATA ON
HEAT-TREATMENT
+------------------------------------+---------+---------+-----------+
| Heat No. | 1 | 2 | 3 |
+------------------------------------+---------+---------+-----------+
|Carbon, per cent | 0.45 | 0.52 | 0.50 |
|Manganese, per cent | 0.68 | 0.62 | 0.47 |
|Decalescent point, degrees F | 1400 | 1425 | 1390 |
|Quenching temperature, degrees F | 1450 | 1475 | 1450 |
|Temperature of oil, degrees F | 160 | 160 | 120 |
|Resultant hardness, scleroscope No |65 to 75 |65 to 75 | *39 |
|Temperature of water, degrees F | | | 75 |
|Resultant hardness, scleroscope No | | | 55 to 60 |
|Tempered until showing a scleroscope| | | |
| hardness of | 48 | 48 | 52 |
|Yield point, tons | 47.8 | 48.6 | 46.5 |
|Breaking point, tons | 67.9 | 65.4 | 66.2 |
|Elongation, per cent | 14.5 | 16.9 | 17.4 |
+------------------------------------+---------+---------+-----------+
_Machinery_
* Note: This shell was then reheated and quenched in water with results
shown.
Referring to results presented in Table II, “Heat No. 3,” it will be
observed that the manganese is only 0.47 per cent with carbon 0.50 per
cent. Comparing “Heat No. 3” with “Heat No. 1”, it is evident that an
increase of 5 points carbon is more than offset by a reduction of 21
points in the manganese. Increase of temperature seemed to offer the
greatest possibilities and sample shells were drawn every 12¹⁄₂ degrees
up to 1675 degrees F. The greatest hardness was obtained at 1637¹⁄₂,
scleroscope readings of from 50 to 55 being the average. This was not
considered satisfactory, and the oil-circulating pump was speeded
up. Scleroscope readings as high as 65 were frequently obtained at a
quenching temperature of approximately 1635 degrees, and when the shell
was tempered to read 48 to 52 on the scleroscope, three test pieces
from one shell gave the results presented in Table III. A careful study
of this data revealed the fact that, while a low-carbon, low-manganese
steel hardens satisfactorily within a limited range of temperature, a
medium steel has a wider range, and a high-carbon steel, a still wider
range of hardening temperature.
TABLE III. RESULTS OF TESTS ON SAMPLES TAKEN FROM A SHELL WITH A
SCLEROSCOPE HARDNESS NUMBER OF FROM 48 TO 52
+--------+---------------------+-------+---------+-----------+
|Heat No.|Scleroscope reading |Yield |Breaking |Elongation,|
| |on test piece after |Point, | point, | per cent |
| | machining | tons | tons | |
+--------+---------------------+-------+---------+-----------+
| |Outside 52--53--50 | | | |
| 1 |Inside 55--55--55 | 55.8 | 73.3 | 14.3 |
| | | | | |
| |Outside 52--54--50 | | | |
| 2 |Inside 55--57--53 | 53.8 | 72.4 | 17.4 |
| | | | | |
| |Outside 57--57--49 | | | |
| 3 |Inside 60--62--51 | 52.8 | 77.3 | 12.7 |
+--------+---------------------+-------+---------+-----------+
_Machinery_
When the shipment of mixed heats previously referred to was treated,
the method pursued was to take 0.50 per cent carbon and 0.50 per
cent manganese as a base composition which hardened at 1600 degrees
F. to show 55 to 65 hardness on the scleroscope. Then: (a) If, for
every point of carbon below 50, there be present 1 or more points of
manganese above 50, the steel should harden satisfactorily at 1600
degrees F. (b) If, for every point of manganese below 50, there be
present 2 or more points of carbon above 50, the steel should harden
satisfactorily at 1600 degrees F. (c) If both carbon and manganese be
below 0.50 per cent, increase the hardening temperature 12¹⁄₂ degrees
F. for each point of manganese short of 50, and 6¹⁄₄ degrees F. for
each point of carbon short of 50. (d) If both carbon and manganese
are above 0.50 per cent, a hardness number above 55 will probably be
obtained at a quenching temperature of 1600 degrees F., but the maximum
hardness, _i.e._, from 75 to 80, will be obtained at a somewhat lower
temperature, the exact temperature being most easily found by starting
at 1500 degrees F. and trying a couple of sample shells every 25
degrees F. until a maximum hardness is obtained. Forgings containing
from 0.50 to 0.55 per cent carbon and from 0.54 to 0.62 per cent
manganese in any varying proportions may be hardened at 1600 degrees
F. to show a hardness number of from 55 to 75; and when tempered to
give a hardness number of from 48 to 52 they will yield the following
results: yield point, 45 to 50 tons; breaking point, 65 to 70 tons; and
elongation, 14 to 20 per cent.
[Illustration: Fig. 12. Chart showing Hardening Temperatures for
Various Percentages of Carbon and Manganese in Steel used for Shrapnel
Shells]
Looking back, (c) offers a basis for charting the hardening points
in a fairly approximate manner, to form a guide as to where the
best hardness may be obtained. Such a chart is shown in Fig. 12.
By following the horizontal and vertical lines from the carbon and
manganese content until they intersect, a diagonal line will be found
which will indicate the temperature at or about which the maximum
hardness will be obtained. This does not prevent the use of 1600
degrees F. as the average temperature for the majority of shells,
provided they are strong enough when hardened at that temperature;
but where shells do not harden satisfactorily at 1600 degrees F., the
chart offers an alternative method subject to such variation as may
arise due to the use of steel from different makers, etc. Probably the
best practice is to make careful scleroscope readings of each piece
before pulling. Care must be taken to have a uniform surface on both
sides, all tool marks being removed with fine emery cloth. The points
tested are shown at _A_, _B_, and _C_ in Fig. 11. After the test piece
is made, the value of the hardness number increases as a result of the
piece being solidly supported in the scleroscope, whereas, when the
reading is made on the shell, the arched form of the wall acts as a
spring, and absorbs the shock to some extent. Readings thus increase
from 2 to 10 points after the test piece is finished.
TABLE IV. DATA ON THE HEAT-TREATMENT AND STRENGTH TESTS OF SHRAPNEL
SHELLS
+--------+----------+------------+-----------+------------+-------+----------+-------------+
| | | Quenching | Tempered, | | | | |
|Carbon, |Manganese,|temperature,|scleroscope|Readings of | Yield | Breaking | Elongation, |
| per | per | degrees | hardness |scleroscope | point,| point, | per |
| cent | cent | F. | No. | | tons | tons | cent |
+--------+----------+------------+-----------+------------+-------+----------+-------------+
| 0.50 | 0.47 | 1635 | 51 | 60-57-57 | 48.3 | 69.9 | 16.9 |
| | | | | 47-48-48 | | | |
| | | | | | | | |
| Three pieces from one shell | | 60-56-53 | 45.2 | 70.6 | 19.1 |
| | | 48-52-58 | | | |
| | | | | | |
| | | 63-56-57 | 51.6 | 74.6 | 16.9 |
| | | 51-55-54 | | | |
| | | | | | |
| 0.48 | 0.65 | 1565 | 49 | 51-54-52 | 47.3 | 67.4 | 15.9 |
| | | 48-53-50 | | | |
| | | | | | |
| Three pieces from one shell | | 51-52-49 | 48.2 | 67.9 | 15.3 |
| | | 53-51-51 | | | |
| | | | | | |
| | | 52-55-50 | 49.2 | 70.7 | 15.4 |
| | | 50-55-47 | | | |
| | | | | | | |
| 0.50 | 0.57 | 1600 | 50 | 50-52-50 | 46.0 | 64.8 | 19.0 |
| | | | | 49-50-49 | | | |
| | | | | | | | |
| 0.50 | 0.57 | 1600 | 50 | 56-60-57 | 55.8 | 77.8 | 14.3 |
| | | | | 54-56-54 | | | |
| | | | | | | | |
| 0.50 | 0.57 | 1600 | 50 | 59-60-56 | 60.7 | 82.2 | 12.7 |
| | | | | 55-59-56 | | | |
| | | | | | | | |
| 0.60 | 0.57 | 1600 | 50 | 60-61-55 | 57.8 | 80.0 | 12.6 |
| | | | | 60-62-57 | | | |
| | | | | | | | |
| 0.60 | 0.57 | 1600 | 52 | 57-57-56 | 48.2 | 69.7 | 17.5 |
| | | | | 54-56-53 | | | |
| | | | | | | | |
| 0.50 | 0.57 | 1600 | 50 | 48-52-50 | 44.2 | 64.3 | 17.4 |
| | | | | 49-52-49 | | | |
| | | | | | | | |
| 0.50 | 0.57 | 1600 | 50 | 52-55-55 | 44.7 | 65.2 | 14.7 |
| | | | | 60-51-52 | | | |
+--------+----------+------------+-----------+------------+-------+----------+-------------+
_Machinery_
A careful study of the data presented in Table IV reveals the
fact that results are not always consistent. With an increase of
carbon, one occasionally finds an increase in elongation and _vice
versa_; and the results due to variations in manganese content are
similarly unreliable. In order to secure a degree of uniformity in
hardness, which will be sufficient to insure test pieces standing up
successfully, it is necessary to have the shell hard inside as well as
outside, and a method of doing this is referred to later. Assuming now
that the shell has been tempered, it is rough-polished on a canvas
buffing wheel around the outside of _B_, Fig. 11, for a width of at
least 1 inch. Readings by the scleroscope are made on a zone ³⁄₄ inch
wide, and if they are between 46 and 52 the shell may be relied upon
to show good results in the tensile test. In making test pieces, it
is desirable to cut the piece from a spot which reads 48 to 50; and
in machining the test piece, care should be taken to remove an equal
quantity of metal from either side of the wall so that the test piece
is a true specimen of the average wall structure. Where a shell is
carelessly quenched, and the test piece so machined that the surface
on one side is practically the same as the inner side of the wall, the
results would not be a true indication of the real average strength,
and a lot of shells might possibly be rejected on account of a slight
oversight in this respect. Reference has been made to the base _A_,
Fig. 11. Forging defects show up here occasionally and in such cases
the shell is at once condemned. These flaws take the form of small
cracks, from the width of a hair up to ¹⁄₁₆ inch. They seldom can be
detected until after heat-treating, and are most easily observed by
polishing the base on a disk grinder. Losses in this respect vary, but
might average about 0.20 per cent. The hardness of the base itself may
vary from 38 to 50, which insures an ample degree of toughness and
avoids all possibility of the shell cracking under fire.
[Illustration: Fig. 13. Lay-out of Heat-treating Department for a
Factory Producing from 12,000 to 15,000 Shrapnel Shells a Week]
=Heat-treating Department.=--Many methods of heating, quenching,
annealing, and cleaning are in use by the different firms engaged in
shell making. For rapidity of output, cleanliness of the resulting
product, ease and economy of operation, and uniformity and control of
results, the lead bath seems best for hardening, and the semi-muffle
furnace for annealing. In one case the use of a lead bath by a skilled
operator yielded excellent results both as to economy and uniformity,
but, when the output exceeds 500 shells per 12 hours, a semi-continuous
furnace meets the requirements to better advantage. The lay-out of a
hardening room for an output of 12,000 shells per week is given in
Fig. 13. The lead baths consist of a rectangular pot of suitable
capacity, resting on a 4¹⁄₂ inch hearth built of common firebrick and
heated by either oil or gas burners below the hearth. They are built
in pairs with a common wall between, which is thick enough to provide
a flue to carry off products of combustion. The quenching tanks are
rectangular, water-jacketed, and provided with two quenching cradles
each. These cradles are arranged to swing lengthwise in the tank, and,
when the carrier holding the shell is lowered into the oil, a pipe is
automatically extended downward into the shell and introduces cold oil
in the inside of the shell, while the operator swings the cradle back
and forth in the tank, thus cooling the outside of the shell at the
same time. This method of quenching made it possible to harden shells
which, by reason of low carbon and manganese, defied all conventional
methods of dipping and swinging back and forth with tongs. The output
per man with this apparatus is largely in excess of any hand method,
while the uniformity and degree of hardness is all that could be
desired.
[Illustration: Fig. 14. Special Arrangement of Scleroscope for Testing
Shrapnel Shells]
[Illustration: Fig. 15. Closing-in Nose of Shrapnel Shell in Hydraulic
Press]
The oil pump draws the oil from a depth of 6 inches below the surface
and pumps it through 100 feet of 1-inch copper pipe arranged in two
50-foot coils in parallel. The cooled oil is delivered into an overhead
reservoir, the overflow being connected to both tanks equally. After
quenching, the shells are set on draining racks, and then washed in
boiling water and sal-soda, placed on another draining rack and then
brushed with wire brushes previous to tempering. The tempering furnace
is of rectangular form, and consists of a long flat hearth with rails
laid lengthwise on it. At each end a space is partitioned off from the
body of the furnace, by means of vertical sliding doors; and a rack
holding a number of shells is deposited on the rails at the front end
of the hearth, the door is elevated and the rack is slid into the main
chamber. After a suitable lapse of time another rack is introduced,
and so on until the first rack is ejected at the rear end of the
furnace. The shells are now hot enough to loosen all foreign matter on
the surface, and a few seconds brushing with a wire brush cleans out
the driving band groove, and leaves the shell with a delicate brown
oxidized finish. The shell is now spotted on three places with a canvas
buff and tested for hardness. Fig. 14 shows the arrangement of the
scleroscope. The shell is supported on a single narrow V-block with
hardened edges, situated immediately under the set-up point. A narrow
strip supports the open end of the shell, thus giving a three-point
support, while a vertical stop at the back of the shell maintains it
in a position tangential to the radius of the swinging arm. The usual
rubber bulb was soon dispensed with as being quite unsuited for such
hard service, and a small pump cylinder substituted. The piston in the
cylinder is operated by a downward pressure of the heel on the pedal to
give compression, and a spring inside the cylinder gives the necessary
pull when the scleroscope hammer is to be raised by suction. After
being tested the shells are ready for “nosing-in.”
[Illustration: Fig. 16. Third Operation on Nose of Shrapnel
Shell--Turning, Facing, and Threading]
[Illustration: Fig. 17. Grinding Shrapnel Shells in One Operation in a
Ford-Smith Grinding Machine carrying a Wheel about 8¹⁄₄ Inches Wide by
20 Inches in Diameter, rotated at 1200 Revolutions per Minute]
[Illustration: Fig. 18. Closing-in Copper Band on Shrapnel Shell in a
Machine provided with Six Dies, as shown in Fig. 20, back of each one
of which there is a Hydraulic Cylinder]
=Closing-in the End of the Shell.=--On some makes of shells,
particularly the British, the nose is closed in before performing the
third series of machining operations. The closing-in is generally
accomplished in a hydraulic or power press. Fig. 15 shows the
closing-in operation being performed in a vertical hydraulic press
capable of exerting a pressure of 800 pounds per square inch. Before
closing the open end of the shell, it is heated in the lead bath, shown
to the left of the illustration, which is kept at a temperature between
1450 and 1500 degrees F. The steel diaphragm, which is larger in
diameter than the nose of the shell, is first thrown in. Then the shell
is placed in the press, and a cone-shaped die descends, closing-in the
nose to the proper shape and diameter. The third machining operation
consists in finishing the radius on the nose, both inside and outside,
and cutting the thread. This is done, as shown in Fig. 16, in an
ordinary engine lathe with a turret on the saddle. The boring is done
with cutters held in boring-bars and the thread cut with a Geometric
collapsible tap. The thread on the 18-pounder is 2.94 inches in
diameter, 14-pitch, Whitworth type.
[Illustration: Fig. 19. Special Type of Wheel-truing Device used on
Ford-Smith Grinding Machine shown in Fig. 17]
=Grinding Shrapnel Shells.=--The exterior surface of a shrapnel shell
is straight for a portion of the length and then curved on the nose.
While the limits required are not extremely close, it is necessary,
where large production is required, to accomplish the finishing
operations on the exterior of the shell in some way by which fairly
close dimensions can be secured as well as large production. Grinding
has, therefore, been recommended for finishing the exterior of the
shell. One method of grinding shrapnel shells, in which a wide-faced
wheel is used that covers the entire ground surface, is shown in Fig.
17. This machine is built by the Ford-Smith Machine Co., Hamilton,
Ont., and carries a wheel about 8¹⁄₄ inches wide by 20 inches in
diameter. The grinding wheel is rotated at 1200 R. P. M., and the work
at 50 R. P. M. The depth of the cut is about ¹⁄₃₂ inch, and the time to
complete one shell varies between two and three minutes. For grinding,
a plug is screwed into the open end of the shell. This is held on the
tailstock center and a chuck holds and drives the shell from the other
end.
[Illustration: Fig. 20. Close View showing Closing-in Dies of Banding
Machine shown in Fig. 18]
It is necessary, of course, that the wheel be kept the correct shape,
and for this purpose an interesting type of wheel-truing device,
differing considerably from that shown in Fig. 17, is now used.
Referring to Fig. 19, it will be seen that this comprises a combination
wheel guard and bracket, the latter being used as a base for the
wheel-truing device proper. The diamond _A_ is carried in a holder _B_
that operates in a slide in the face of the traversing wheel-truing
slide _C_. The diamond holder carries a cam point _D_ which is kept in
contact with the guide or former cam _E_ by means of a spring _F_. The
wheel-truing slide _C_ is traversed by a triple pitch screw _G_ so as
to give a rapid movement to the slide in order to produce what might be
termed a “rough-truing” of the wheel. For change in diameter, and also
for bringing the diamond in contact with the wheel, a vertical slide
_H_ is provided that is operated by handle _I_. In order to observe the
diamond when truing the wheel, a trap door _J_ is provided in the wheel
guard, which can be dropped down into place when the actual grinding of
the shell is being done.
=Pressing on the Rifling Band.=--In order to rotate the shrapnel when
propelling it out of the howitzer, it is necessary to put on a rifling
band to take the rifling grooves of the gun bore. As a rule, these
rifling bands are made from copper tubing and are simply cut off in a
hand screw machine or turret lathe. The next operation is to close in
the rifling band on the shrapnel shell. The ring is dropped over the
shell and a fixture is used to locate it in the correct relation to
the groove in the circumference of the shell. Then a slight pressure
is exerted on it to align it properly in the groove. It is now placed
in the banding machine shown in Fig. 18. This particular machine is
provided with six dies as shown in Fig. 20, and back of each one is
a hydraulic cylinder operated by water pressure. Two squeezers are
necessary to close the rifling band properly into the groove, the shell
being given a half turn after each squeeze.
[Illustration: Fig. 21. Shrapnel Banding Machine built by the West Tire
Setter Co., having a Capacity for Compressing two Bands per Minute]
There are several different machines on the market for performing this
closing-in operation on the rifling band. Another machine, built by
the West Tire Setter Co., Rochester, N. Y., is shown in Fig. 21. The
principle upon which this machine operates is almost identical with
that previously described, but in this case oil is used as a pressure
medium. It is forced into the machine by means of a belt-driven pump
shown to the left of the illustration, which drives the oil from the
oil tank and carries it to the center of the base of the press. An
oil head is located at this point from which the pipes are run to
each of the six rams or cylinders. The amount of pressure required
for compressing the copper band depends largely upon the width and
thickness and the amount that the band must be spread to fill the
grooves, rather than upon the diameter of the shell. The machine
shown in Fig. 21 is capable of exerting a pressure of 30 tons on each
cylinder or a combined pressure of 180 tons on all six cylinders. It
has a capacity for compressing at least two bands per minute.
[Illustration: Fig. 22. Assembling Bullets, Resin, and Fuse Socket in
Shrapnel Shell]
[Illustration: Fig. 23. Finishing Rifling Band on Shrapnel Shell to
Shape]
=Machining the Rifling Band.=--One method of machining the rifling band
to the correct shape is shown in Fig. 23. Here a Fox lathe is used
which is provided with a chuck for holding the shell and which carries
in the turret a revolving center for additionally supporting it. The
machining is done by form tools which are of the correct shape. Before
any other machining operations can be accomplished it is necessary
to put in the tin powder cup, brass fuse tube, bullets, and resin.
This cup is slipped in past the steel diaphragm, then both parts are
allowed to drop to the bottom and the fuse tube is screwed into the
diaphragm. The required number of lead bullets, which for the British
18-pound shrapnel is about 375 per shell, is then poured in. The
bullets are held in a tank and are allowed to flow out upon the opening
of a stopcock. In order to pack the bullets solidly, a compressed air
ramming device forms the base upon which the shell rests while the
bullets are being poured in. This is operated three or four times for
the filling of each shell and arranges the bullets compactly.
[Illustration: Fig. 24. Illustration showing some of the Principal
Gaging Operations on Shrapnel Shells]
[Illustration: Fig. 25. 18-pound Shrapnel Shell showing Dimensions and
Manufacturing Limits]
The resin is now poured in, as shown in the center of Fig. 22. This
is carried in the tank which is heated by a gas furnace and is poured
in almost level with the top of the bullets. The shell is then placed
on the scale in the immediate foreground and weighed. One dram plus
or minus is allowed as a variation, and in order to not exceed this,
more or less resin is poured in until the correct weight is obtained.
The brass fuse socket is now screwed in as shown to the left of the
illustration, and upon the completion of this operation the shell is
ready for the fourth and last machining operation. This last operation
consists in machining the brass socket on the outside diameter to
conform to the radius on the nose of the shell, and boring on the
inside and threading to fit the fuse body. These operations are handled
in a Fox brass working lathe. Upon the completion of the machining
operations the plug is screwed in, the shell stamped, cleaned, weighed,
and inspected by government inspectors. After this, the shell is given
two coats of paint and a red band is painted around the nose. It is now
packed in boxes holding six shells and is ready for shipment. This
completes the manufacture of the shrapnel shell.
[Illustration: Fig. 26. Group of Gages made by Wells Bros. Co. for
gaging British Shrapnel Shells and Parts]
[Illustration: Fig. 27. Diagram showing Application of Wells Bros.
Gages]
=Gaging Shrapnel Shells.=--The machining operations on shrapnel
shells are required to be held within certain limits, and government
inspectors watch these closely. Some of the principal gaging operations
on the shrapnel shell body are shown in Fig. 24. Fig. 25 shows the
18-pound shrapnel shell in section, and gives the principal dimensions
together with the limits; it will be seen from this illustration that
the range allowable is in most cases large. The Wells Bros. Co.,
Greenfield, Mass., has made a large number of shrapnel gages, some of
which are shown in the accompanying illustrations. In the three upper
views of Fig. 24, the Wells Bros, standard thread gage is illustrated.
This is used for all diameter measurements by substituting flat gaging
pins for the V-points used when gaging thread diameters.
[Illustration: Fig. 28. Collection of Wells Bros. Co.’s American
Shrapnel Shell Gages]
[Illustration: Fig. 29. Dwight-Slate Hand-operated Marking Machine for
Shrapnel Shells]
=Gages for British Shrapnel Parts.=--Fig. 26 illustrates typical gages
for gaging such parts of the British shrapnel as body diameters,
diaphragm seat, powder pocket, fuse socket, thread diameters, and fuse
parts. Fig. 27 shows the application of several different types of
shrapnel shell gages. At _A_ is the gage for the over-all length. At
_B_ is the gage used for measuring the thickness of the closed end.
The outer arm of this gage can be swung away to allow the placing of
the gage on the standard. At the extreme lower left-hand corner of the
gaging arm is a slight shoulder on the rod and the height of this acts
as the limit. _C_ shows the application of outside diameter and thread
gages. _D_ shows three form gages for checking the shape and dimensions
of the wave ribs, the diameter and shape of the undercut in the band
groove, and the shape of the nose of the shell. _E_ shows the gage
used for checking the thickness of the wall of the shell at different
distances from the mouth. _F_ shows the application of a powder pocket
gage, and also a gage for checking the shape of the finished rifling
band.
[Illustration: Fig. 30. Power-driven Dwight-Slate Marking Machine for
Shrapnel Shells]
=Gages for American Shrapnel Shells.=--Fig. 28 shows a miscellaneous
collection of gages used in checking the dimensions of the American
shrapnel shell. Gages, _A_, _B_, _C_, and _D_ are for measuring the
diameter of the diaphragm seat. _E_ is for checking the distance from
the diaphragm seat to the mouth end of the shell, and gage _F_ is for
the outside diameter of the shell. Gage _G_ is used for the rifling
band groove. Gages _H_ and _I_ are for the thread in the mouth of the
shell, _H_ being a “not-go” and _I_ a “go” gage.
The gage at _J_ performs several gaging functions on the American
shell. It consists of a standard having two upright posts across which
a bar is mounted. The purpose of the bar is to gage the over-all
length of the shell, and its lower surface is provided with two steps
giving the limits. This gage is also used for measuring the depth of
the powder pocket, rod _K_ and block _L_ performing this function. Two
rings are cut around the rod _K_ registering with the top surface of
the bar, the purpose being to show the accuracy of the work.
Another interesting gage is shown at _M_. This is for gaging the
concentricity of the shell and consists of an arbor mounted so that it
can be swung on a pivot. The arbor carries two collars _N_ and _O_ that
fit in the shell. Collar _P_ is merely a sizing plug and when the gage
is in use this plug is removed. A gaging finger _Q_ rests against the
shell when it is on this arbor, and a standard type of indicator _R_
shows the variation in concentricity when the gage, collars, and shell
are rotated on the arbor.
=Marking Shrapnel Shells.=--All shrapnel shells are marked on their
circumference with five or six lines of lettering, as shown in Fig. 29.
This indicates the size of the shell, the series, muzzle velocity, name
of the manufacturer, date completed, etc. Two types of machines for
producing the stamping, built by Noble & Westbrook, Hartford, Conn.,
are shown in Figs. 29 and 30. The machine shown in Fig. 29 is of the
hand-operated type. The figure block _A_ is held in a slide that is
moved longitudinally by pulling down handle _B_, rolling the shell, and
at the same time stamping it. The shell is located on the table in the
two positions by gages _C_ and _D_.
The “Dwight-Slate” stamping machine shown in Fig. 30 is power-driven,
and the work is held on an elevating table. The stamp is held in a
slide operated by an eccentric and connecting-rod. In this machine the
shell is not distorted.
CHAPTER IV
MACHINES AND TOOLS FOR SHRAPNEL MANUFACTURE
=Reed-Prentice Co. Equipment for Machining Forged Shrapnel Shells.=--In
machining the 18-pound British shrapnel shell on the equipment
furnished by the Reed-Prentice Co., Worcester, Mass., eight distinct
operations are performed as follows: First, drilling a center hole
in the closed end of the forging in a Prentice 16-inch ball-bearing
sensitive drilling machine equipped with a special centering fixture;
second, rough-turning the outside diameter, grooving, squaring the
closed end and rounding the corners in a Reed-Prentice 14-inch heavy
type automatic lathe; third, machining the powder pocket and diaphragm
seat, as well as the internal and external diameters of the nose in
a 14-inch Reed extra-heavy turret lathe; fourth, under-cutting band
grooves and producing wave ribs in a 14-inch Reed engine lathe; fifth,
boring, reaming, threading and facing the open end in a Reed 14-inch
extra-heavy turret lathe; sixth, finish-turning outside diameter and
radius on nose, also form-turning copper band in a Reed 14-inch heavy
type automatic lathe; seventh, cutting off center projection on closed
end of shell in a Reed 14-inch engine lathe; eighth, finishing brass
socket to form, cleaning inside of socket and cutting off excess length
of tube in a Reed 14-inch extra-heavy turning lathe.
=First Operation on Rough Shell Forging.=--The drilling of the center
hole in the closed end of the forging is a comparatively simple
operation, and is performed in an interesting fixture held on a 16-inch
Prentice ball-bearing sensitive drilling machine. This fixture, which
is designed for handling the work quickly, is shown in Fig. 1, and
consists of the base casting _A_ clamped to the table of the drilling
machine. The entire back part of the jig swings on the trunnion _B_ to
provide a means for quickly removing the forging _C_ from the arbor
_D_. A locking-pin _E_ is used for locating the fixture in its upright
position for drilling. Bushing _G_ in the top plate _F_ of the fixture
guides the combination drill and countersink.
[Illustration: Fig. 1. Fixtures used for holding Shrapnel Shell
Forgings when drilling Center Hole in a 16-inch Prentice Ball Bearing
Sensitive Drilling Machine]
The construction of the work-holding arbor is worthy of special
attention. This arbor _D_ has a cap _H_ on its top end that acts as a
stop for the inside of the forging, which, in being placed over the
arbor, is located centrally and clamped by fingers _N_. To operate
these fingers, hand lever _I_ is depressed, and as this is fulcrumed
at the point _J_, it causes collar _K_ to rise on the arbor. Yoke _L_
forms a connection between the lever and the collar with which the
sleeve carrying fingers _N_ is integral. Fingers _N_ are fulcrumed in
arbor _D_ and are thrown outward to grip the forging when sleeve _M_
is raised. Light springs _O_ tend to keep the gripping fingers in a
vertical position against the arbor when they are not being forced
outward by the inclined surfaces on sleeve _M_. Handle _I_ carries a
spring pawl _P_ that holds the sleeve _M_ stationary while the forging
is being center-drilled.
[Illustration: Fig. 2. Tool Lay-out for performing Second Series of
Operations on Reed-Prentice Heavy Type Automatic Lathe]
=Second or Rough-turning and Facing Operations.=--The second operation
is performed on a Reed-Prentice 14-inch heavy type automatic lathe,
as shown in Figs. 2 and 3. The forging _A_ is held on an internal
expanding arbor _B_, the driving part of which is supported by
the head-center. At the closed end, the shell is steadied by the
tail-center. The bottom of the shell rests against the end of the
arbor which acts as a gage. In this setting, the external diameter of
the forging is rough-turned by four tools _F_, mounted on the carriage
_G_. This carriage has a travel slightly less than two inches, and an
automatic throw-off is provided at the end of the cut that disengages
the tools, draws them back and returns the carriage. At the rear of
the carriage on this machine a facing arm is mounted on a heavy bar.
Turning tools are carried on this facing arm, as shown, and when the
front carriage feeds longitudinally a cam bracket _O_, bolted to the
carriage, is carried along with it. Clamped on this bracket is an
adjustable cam _N_ held in place by screws. Cam roll _M_ on the facing
arm contacts with cam _N_, causing the facing arm to rock forward as
the carriage travels longitudinally.
[Illustration: Fig. 3. Section through Reed-Prentice Automatic Lathe,
showing Tool Arrangement]
Referring to the plan view in Fig. 2, tool _H_, held in the arm, faces
the end of the forging, tool _I_ chamfers the corner, and tool _J_ cuts
the depression for the wave ribs, leaving a projection in the center
from which the ribs are formed. It should be understood that the tools
on the carriage and facing arm work together. One man can run two of
these machines without trouble.
=Third Series of Machining Operations.=--The third series of operations
on the shrapnel forging is performed on a 14-inch Reed heavy lathe with
a specially large turret, as shown in Fig. 4. This lathe is fitted
with a 12-inch three-jaw chuck, bored out to 3¹⁄₂ inches to permit
the forging to extend into it. The forging _A_ is put in the chuck
as shown at _B_, and the jaws grip at _C_. The first operation is
performed with a bar _D_ carrying a blade cutter _E_ that rough-bores
the powder pocket, and tool _F_ that rough-bores the mouth. The turret
is now indexed, and a boring-bar carrying a blade _G_ roughs out the
diaphragm seat, while an auxiliary tool _H_ faces the shell to length.
At the next indexing of the turret the boring-bar _I_ that carries the
finishing tool _J_ finishes the diaphragm seat and powder chamber.
[Illustration: Fig. 4. Tooling Equipment for performing Third Series of
Operations on 14-inch Extra-heavy Turret Lathe]
[Illustration: Fig. 5. Tools used for Under-cutting and Waving Band
Grooves on Reed 14-inch Engine Lathe]
=Fourth Operation--Under-cutting and “Waving” Band Groove.=--For the
fourth operation, the forging is held in a 14-inch Reed engine lathe
provided with an automatic attachment for under-cutting and waving the
ribs for the copper band. The tool equipment used is shown in Fig. 5,
where _A_ is the forging held by one end in the chuck and supported
on the opposite end by the tail-center. The tools are all located in
holders on the heavy base block _B_, and their operation is controlled
from the carriage _R_ of the lathe. The cutting of the wave ribs is
done by tool _C_ at the front, held on a slide that operates on the
top of block _B_. Spring _D_ keeps the roll _E_ on the lower slide of
the tool-holder in contact with the cam slot in cam-plate _F_ that is
fastened to carriage _R_. When the carriage is traversed toward the
chuck, the irregular surface of cam-plate _F_ engages the roll and
forces the tool-holder forward. Side motion to produce the wave is then
effected by face-cam _G_, mounted on the chuck and contacting with the
roll _H_. This roll is supported on a bracket forming an auxiliary
slide _S_ that carries the waving tool _C_. A stiff barrel spring keeps
slide _S_ in contact with the cam _G_. Thus, when the machine spindle
revolves, the auxiliary slide is caused to oscillate back and forth far
enough to give the desired amount of wave.
The under-cutting in the band groove is accomplished by tools _I_ and
_J_ which are mounted on separate tool-slides _K_ and _L_. These slides
are fed in at an angle to the axis of the forging, against the action
of coil springs _M_ and _N_, by the cam surfaces of plate _Q_ in which
rolls _O_ and _P_ work. Plate _Q_ is bolted to carriage _R_ which, in
advancing toward the chuck, forces in the under-cutting tools in the
manner just described. The tail-center of this machine is fitted with a
quick-acting mechanism so that it may be withdrawn quickly to insert a
new piece.
=Fifth Series of Operations.=--Before performing the fifth series of
operations, the forging is heated and closed in on the nose. It is then
handled in the following manner: A Reed 14-inch heavy lathe, equipped
with an extra large turret mounted on a special wide-bridge carriage
carries tools for boring, reaming, threading and final squaring of the
open end, as shown in Fig. 6. The shell forging for these operations
is held in a three-jaw chuck provided with special jaws. In the first
position the rough-boring of the nose and the rough-facing of the
extreme end is performed with tools _B_ and _C_. The turret is then
indexed and tools _D_ and _E_ finish-ream the hole in the nose and face
the end. The tap _F_ is next brought into position, cutting the thread
in the nose.
[Illustration: Fig. 6. Turret Tools held on Reed 14-inch Extra-heavy
Lathe for performing Fifth Series of Operations]
The turret is again indexed, bringing a special form boring tool into
position. Here the boring tool _G_ is carried in a bar _H_ held in a
holder of the cross-sliding carriage type that is fastened to two faces
of the turret. By means of cross-screw _J_, the boring tool _H_ may be
drawn in or out at will. This tool operates as follows: As the turret
is advanced, handle _J_ is operated to let tool _G_ enter the nose of
the shell, and, upon the continued advance of the turret, arrow head
_M_ is forced in between and gripped by the fingers _N_. The turret is
now backed away from the chuck, and while receding acts upon slide _P_
through the medium of roll _L_ and cam groove _R_. The plate containing
cam groove _R_ is attached to the arrow head _M_ and consequently is
held stationary while the turret is being withdrawn from the work. This
backward movement of the turret is continued until the tool _G_ is
withdrawn from the work and slide _S_ comes in contact with check-nuts
on rod _O_, withdrawing arrow head _M_ from fingers _N_ and allowing
the turret to be indexed ready for the first operation on the next
forging.
[Illustration: Fig. 7. Reed-Prentice 14-inch Heavy Type Automatic Lathe
used for performing Sixth Series of Operations]
=Sixth or Finish-turning Operations.=--The sixth series of operations
is performed on a Reed-Prentice 14-inch heavy type automatic lathe,
similar to that used for the second operation, and the machine is
also operated in a manner similar to that previously described. The
operations consist in finish-turning the outside diameter of the shell
and turning the radius on the nose. In addition, the copper rifling
band, put on previous to this operation, is turned to shape. Referring
to Fig. 7, the shrapnel shell _A_ is held by the tail-center at one end
and is supported and driven from the other end by a plug screwed into
it. This plug is held on the live center and is driven by an equalizing
driver, coming in contact with pins in the special faceplate.
[Illustration: Fig. 8. Tools for machining Brass Fuse Socket on 14-inch
Heavy Turning Lathe--Eighth Operation]
Two slides _B_ and _C_ are carried on the front of the carriage. Slide
_C_ carries three tools _D_; two of these start in from the rifling
band and turn in toward the nose, and the other works up toward the
rifling band from the closed end. Tool _E_, carried in slide _B_,
turns the curve on the nose of the shell and is controlled in its
action by means of a slot in cam _F_ in which a roller held to the
slide operates. At the rear of the carriage is carried a facing bar
attachment, as previously described in connection with the second
operation. This attachment carries three tools, as illustrated,
for machining the rifling band to shape, facing the closed end and
chamfering the corner.
=Seventh and Eighth Operations.=--After the sixth operation, the fuse
tube is threaded into the diaphragm, the bullets put in, and the hot
resin poured in to keep them from rattling. The brass socket is then
screwed into the nose and the fuse tube soldered to it. The shell is
now ready for the seventh operation which consists in cutting off the
center projection. This is accomplished in a Reed 14-inch engine lathe,
provided with a faceplate chuck for holding and driving the shell at
the open end, and a steadyrest for supporting it close to the point
where the cutting is being done. The shell is now ready for the eighth
operation, which consists in machining the brass socket to shape in an
extra-heavy lathe as shown in Fig. 8. The tools used for machining are
retained in a special holder on the carriage. Tool _A_, which is used
for facing off the fuse tube and the brass socket, is inverted, starts
at the center and is fed out toward the circumference. The external
surface of the socket is machined with a circular forming tool _C_ held
on a stud _D_ located in block _B_. The inward travel of this tool is
limited by stop _E_ coming in contact with the shell.
[Illustration: Fig. 9. Shrapnel Case made from Chrome-nickel Steel
having High Tensile Strength on a Cleveland Automatic Screw Machine
with Special Tool Equipment]
[Illustration: Fig. 10. Order of Operations on the Shrapnel Case]
=Making Shrapnel Shells on the Cleveland Automatic.=--An unusual
example of automatic machine work is that of producing the shrapnel
shell shown in Fig. 9. This shell is made from a bar of 3¹⁄₁₆ inch
chrome-nickel steel stock. The steel has a tensile strength varying
from 125,000 to 135,000 pounds per square inch, and is extremely tough.
The work is accomplished on a 3¹⁄₄-inch Cleveland automatic, and the
tooling equipment, as shown in Figs. 10, 11, and 12, is interesting.
While the general operation of the Cleveland automatic is well
understood by many mechanics, the production of this piece illustrates
a number of points in the operation of this machine which are not so
well known. Therefore, it is advisable to explain in detail just how
this interesting job is handled.
[Illustration: Fig. 11. Cleveland 3¹⁄₄-inch Automatic Screw Machine set
up for making a Shrapnel Case in Twenty-five Minutes]
The first operation, as the job was originally laid out, was to feed
the stock out to the stop _A_, shown in Fig. 11, which is held on the
cross-slide and operated by a lever on the base of the machine. This
method has been improved upon since the photograph shown in Fig. 11
was taken, and the time reduced from twenty-seven and one-half minutes
to twenty-five minutes (see Fig. 10 for improved method). The second
operation is to rough-drill the large hole with an inserted bit _B_,
step the hole for the taper reamer with cutter _C_ and rough-turn the
external diameter with cutter _D_ held in a special turning attachment.
This attachment envelops the shanks of all six tools in the turret in
order to obtain support. The cutters in the attachment shown in Fig.
11 work in advance of the under-cutting forming tool _E_ shown in Fig.
12, which is held on the rear cross-slide. The time required for the
completion of the operations outlined is thirteen minutes.
[Illustration: Fig. 12. Showing Tools held on the Front and Rear
Cross-slides for performing the Knurling, Forming, and Cutting-off
Operations on the Shrapnel Case]
In the third operation drill _H_ finishes the powder pocket, and two
cutters _I_ counterbore for the tap--time required three minutes. The
fourth operation consists in finishing the diaphragm seat with the
counterbore _J_, finishing the front end with inserted cutter _K_ and
breaking the corner to facilitate tapping with inserted cutter _L_,
the time required being forty-five seconds. In the fifth operation the
thread is cut with a tap _M_ held in the tap-holder _N_ in forty-five
seconds. Then the turret is indexed and for the sixth operation the
hole is taper-reamed with reamer _O_, provided with four inserted
“Novo” steel blades, in ninety seconds. The last and seventh operation
consists in knurling the band with a knurl _P_ (see Fig. 12) mounted on
the front cross-slide, and cutting off the shell with a cut-off blade
_Q_ retained in a holder on the rear cross-slide--time six minutes.
The total time required to produce this shrapnel case by the improved
methods illustrated by the diagram in Fig. 10 is twenty-five minutes.
There are several points of unusual interest in the production of this
shrapnel case. One is the large amount of stock to be removed to form
the hole; the second is the long taper-reaming operation--difficult
work to accomplish satisfactorily on an automatic screw machine--and
the third is the long outside forming operation which must be held to a
limit of 0.0005 inch on the diameter. In order to accomplish this last
operation successfully, the external diameter of the piece is first
turned with a cutter held in a separate turning attachment, leaving
only 0.010 inch on the diameter to be removed by a wide under-cutting
or shaving tool _E_ held very rigidly on the rear cross-slide. Not
only must the case be exact as regards diameter, but it must not vary
from one end to the other nor at any point throughout its length. The
large shaving tool held rigidly in the manner illustrated in Fig. 12
accomplishes this result satisfactorily.
The material from which the case is made is so tough that some
difficulty was met with in selecting a tool steel that would stand up
for a reasonable length of time under cut. The drills and counterbores
are tipped with “Novo” cutters and all the forming tools, including
the cut-off tool, are also made from the same steel. The only cutting
tool in the entire tooling equipment not made of this steel is the
tap. The bar is rotated at sixty-four revolutions per minute, giving a
surface speed for the external cutting tools of approximately fifty-one
surface feet per minute.
[Illustration: Fig. 13. First Operation on Shrapnel Shell, performed on
a No. 6A Potter & Johnston Automatic Chucking and Turning Machine]
=Machining the British Forged Shell on Potter & Johnston
Automatics.=--In making the British forged shell on the Potter &
Johnston automatic chucking and turning machine, three operations
complete the work. The first operation completes the outside of the
shell, except for the extreme end which is covered by the gripping
mechanism of the chuck. The second operation finishes the inside of the
shell and at the same time finish-turns the extreme open end. After
the second operation is performed the shell is “nosed,” which consists
in heating it in a lead bath and then striking it under a light press
to close in the end. The third operation then follows, and consists in
taking light cuts from the inside diameter and threading the open end
of the shell.
[Illustration: Fig. 14. Expanding Arbor and Chucking Mechanism used
on Potter & Johnston Automatic Chucking and Turning Machines for
performing First Operation on Forged Shrapnel Shells]
[Illustration: Fig. 15. Set-up on a No. 6A Potter & Johnston Automatic
Chucking and Turning Machine for First Operation on Forged Shrapnel
Shells]
=Method of Holding Shell for First Operation.=--For the first
operation, the shell is held on an expanding arbor of the type shown in
Fig. 14. The arbor _A_ is tapered on its rear end and is held in the
nose of the spindle of the machine. The shell is pushed onto this
arbor until the end of the arbor strikes the bottom of the shell. The
gripping mechanism which comprises six jaws _B_ and a draw-in plunger
_C_ is contained inside the arbor. The external diameter of the arbor
is machined to practically the same shape as the internal diameter of
the shell, but is smaller. The jaws are held in slots which control
their movement in every direction except radially. They are forced out
radially by means of the draw-in bar _C_ which is provided with tapered
seats that engage the inward end of the jaws. The bar _C_ is operated
by a hand lever _D_ that extends up over the top of the machine, is
fulcrumed in a bracket on the rear bearing cap, and is connected to a
sliding sleeve _E_.
In clamping the work on the arbor, lever _D_ is lifted up, this action
drawing the sliding collar _E_ to the right along the sleeve _F_,
which, in turn, allows the forward end of the fingers _G_ to close
in. This releases the pressure of the outer end of the fingers on the
draw-in bar _C_. When the pressure from bar _C_ is released by means of
handle _D_, heavy coil springs _H_ then come into action forcing the
draw-in bar back and expanding the clamping jaws. Additional clamping
means are provided by three set-screws which are brought to bear on the
work after it has been clamped in position by the jaws. To release the
work, the reverse action takes place, that is, lever _D_ is forced down
which slides the collar _E_ to the left, operating the fingers _G_,
which, in turn, overcome the pressure of the springs _H_, allowing the
clamping jaws _B_ to collapse.
=First Machining Operation Set-up.=--The order of the first series of
operations in machining a forged shrapnel shell is as follows: First,
rough-turn 7 inches along body of shell, face end and chamfer; second,
finish-turn 2¹⁄₂ inches along shell; third, rough-groove for copper
band and dovetail; fourth, turn waves in groove.
For the first operation, the work is held on the expanding arbor
shown in Fig. 14, and the tool equipment, which is of an unusually
interesting character, is shown in Fig. 15. The first rough-turning
operation, accomplished by turret tool _A_, which is of the relieving
type to be described later, is held on the first face of the turret and
roughs down the body of the shell. On the opposite side of the holder
is a roller support _B_ which supports the shell while the turning tool
is in operation. The end of the shell is faced by means of a facing
tool _C_ which is really a type of facing mill. The end of the shell is
then chamfered by means of a chamfering tool _D_ that removes the sharp
corner.
[Illustration: Fig. 16. Details of Relieving Turning Tool-holder shown
in Fig. 15]
After these operations have been performed, the turret is indexed and
the second face of the turret is brought in line with the chuck. This
operation is accomplished with a relieving tool-holder _E_ carrying a
cutter _e_, which takes a cut 2¹⁄₂ inches along the body of the shell.
An interesting feature of this tool is that on the return stroke of the
turret it swivels back out of the way so that the shell is not scored
by the tool dragging over it. The construction of this tool is more
clearly shown in Fig. 16.
As is clearly shown in this illustration, the turret relieving turning
tool comprises a shank on which is fulcrumed a tool-holding member _B_.
This is slotted out to carry the turning tool _C_ which is clamped
in place by two set-screws _D_ and is adjusted to turn the correct
diameter by means of an adjusting stud and clamping nut _F_ and
_G_. The method of operating this tool is as follows: The fulcrumed
tool-holder _B_ is “held up” by means of a fillister-head screw,
screwed into a stud _H_ and acted upon by a coil spring _I_. A hole to
receive the stud is drilled in the tool-holder _B_, allowing about ¹⁄₁₆
inch clearance. When the tool is in action it has a reverse position
to that shown in the illustration, that is, the turning tool instead
of being parallel with the center line is at a slight angle with it.
In action, as soon as the turret advances, the tool comes into contact
with the work, and the work, turning around, forces the cutting tool
down and consequently depresses the spring, at the same time bringing
the “lower part” of the hole into contact with the extended plug on
the holder. In this way the tool is held rigidly and in contact with
the work. As soon as the turret begins to move back, however, and the
cutting pressure is released, the spring comes into action and throws
up the tool, bringing it out of contact with the work.
Upon the completion of the operation which is accomplished from the
second turret face, the turret is again indexed and the next operation
is performed from the rear cross-slide and the third turret face.
The third operation consists in cutting the grooves for the rifling
band, and, on account of the under-cutting necessary, involves some
interesting points. In order to hold the work rigidly while the
grooving tools are acting on it, a revolving support _F_ is brought
in from the turret. The wide tool _G_ for cutting the band grooves
(this tool removes the greatest amount of the stock) is held on the
rear cross-slide and is of the under-cutting type; that is to say, it
operates under the work or tangentially instead of radially. Held on a
bracket on the third turret face are two tools _H_ and _I_, the purpose
of which is to dovetail the rifling band grooves. These turret tools
are held in a holder working in a slide on the bracket fastened to the
turret face and are operated by a block held on the rear cross-slide.
The action of these three tools, therefore, is simultaneous. The wide
grooving tool, however, is slightly ahead of the dovetailing tools.
[Illustration: Fig. 17. Type of Draw-In Collet and Chucking Mechanism
for holding Forged Shrapnel Shell for performing Second Series of
Operations]
The last operation is accomplished when the turret is indexed to the
fourth position. Here, again, a roller support _J_ steadies the work
while the waving tool is in action on it. The two waves that are formed
are for the purpose of preventing the rifling ring from turning, and
they deviate about ¹⁄₁₆ inch laterally from being a true annular rib.
The tool for cutting these ribs is shown at _K_ and is of the forming
type held in a dovetailed groove in the holder _L_. This also carries
a roll _M_ which contacts with the waved surface of the face-cam _N_,
the curve of which gives the correct out-and-in motions to the waving
tool _K_. The cam face is on a sleeve that is threaded onto the nose of
the spindle of the machine, as is shown to the left of the illustration
opposite the first turret face.
=Method of Holding Shell for Second Operation.=--The second series of
operations on the shell is also performed on the Potter & Johnston
automatic chucking and turning machine. The shell is held at the base
end by a special collet of the draw-in type, as shown in Fig. 17.
Fixed in the nose of the spindle is a positive stop _A_ against which
the shell is held by means of the draw-in collet _B_. This collet
extends into the draw-in rod _C_, to which it is attached. The method
of operating this gripping mechanism differs slightly from that shown
in Fig. 14. In this case the spring collet _B_ is drawn into a tapered
sleeve to clamp it on the work. This is effected by means of lever _D_
which is fulcrumed in a bracket extending from the rear bearing cap of
the machine and operates a sliding cam sleeve _E_. The cam, in turn,
operates fingers _F_, only one of which is shown, the latter acting
upon the draw-in rod _C_ to which the collet is attached. By depressing
lever _D_, the chuck is opened by means of the coil springs _G_ which
act upon the draw-in rod _C_ when the pressure of the fingers has been
released. Lifting up handle _D_ closes the chuck, and depressing it
opens the chuck.
[Illustration: Fig. 18. Tooling Equipment used on No. 6A Potter &
Johnston Automatic Chucking and Turning Machine for performing Second
Series of Operations on Forged Shrapnel Shell]
=Second Series of Machining Operations on Shrapnel Shells.=--The
operations on the shrapnel shell performed in the second setting are
shown in Fig. 18. The relieving tool _A_, held on the first face of
the turret, covers that section of the shell which in the former
operation was held in the gripping jaws. While this cut is being taken,
a turret tool _B_ rough-bores the powder pocket and diaphragm seat.
The relieving tool _A_ is constructed and operated similarly to the
relieving tool described in connection with Fig. 16. It will be noted
here that the threads on the spindle nose are protected by a cast-iron
cap to prevent them from being injured. Upon the completion of the
operation just described, the turret is indexed, bringing the second
face in line with the spindle. Here the diaphragm seat is finished
with a flat cutter _C_, which is held in the boring tool illustrated.
The turret is again indexed into the third position, where the powder
pocket is finished by means of the flat cutter _D_.
The turret is now indexed to bring the fourth face in line with the
spindle where the extreme open end of the shell is turned taper by
means of a tool _E_ that is carried on the front cross-slide and
operated by the turret. By referring to this illustration, it will be
noticed that the taper is turned from the spindle toward the outer
end of the shell and is, therefore, a reverse turning operation. The
tool is caused to move toward the turret by using a rack and pinion to
reverse the movement. On this operation, as well as on the previous
one, one man takes care of four machines.
[Illustration: Fig. 19. Machining Inside of Shrapnel Shell, and
threading with Automatic Collapsible Tap on Potter & Johnston Automatic
Chucking and Turning Machine]
=Third Machining Operation on Shrapnel Shells.=--Before any other
machining operations are done on the shell, it is taken to a lead bath
where it is heated and afterward placed under a press which closes
in the nose or open end of the shell. For machining in the third
operation, the shell is held practically in the same manner as for the
second operation, except that it is gripped farther along the body.
The machining performed in this operation is as follows: On the first
turret face, rough-bore and finish-bore for a distance of 1 inch from
the end of the shell; second turret face, rough-bore the inside of
the shell for a distance of 1 inch back from the thread; third turret
face, finish-form on the inside for a distance of 1 inch back of the
thread; and fourth turret face, thread with a collapsible tap. The
various machining operations on the 3-inch size of shrapnel shells
are performed on a standard Potter & Johnston 6A automatic chucking
and turning lathe. It is recommended that these machines be run in
batteries or units of seven each, four machines being set up for the
first operation, two machines for the second operation, and one machine
for the third operation.
[Illustration: Fig. 20. First Series of Operations on “Frankford” Shell
on a Potter & Johnston 6A Automatic Chucking and Turning Lathe]
[Illustration: Fig. 21. Second Series of Operations on “Frankford”
Shell on Potter & Johnston Automatic Chucking and Turning Lathe]
=Machining “Frankford” Forged Shell.=--The machining of the American
or “Frankford” 3-inch type of high-explosive shrapnel shell is
comparatively easy, inasmuch as there is no nosing to be done, and the
entire shell may be machined at two settings. Fig. 20 shows the way
in which the first operation is taken care of on the No. 6A Potter &
Johnston automatic chucking and turning lathe. The forged shell is held
on an expanding arbor of the same type as that shown in Fig. 15. In
the first turret position, the operations consist in taking a straight
cut across the diameter and facing off the end. The external turning
tool _A_ is of the relieving type, and _B_ is a facing tool that works
on the end. Both of these tools are supported and operated from the
turret. A roll support, not shown, steadies the work while tool _A_
is working. The turret now backs out, and a forming tool, held on
the cross-slide, advances, cuts the rifling band and the semicircular
grooves in the end of the shell, and at the same time chamfers the
corner. Knurl _D_, held on the rear of the cross-slide, is then
advanced. This knurls the bottom of the rifling band groove.
By referring to Fig. 20, it will be seen that the grooves do not
extend entirely across the face of the knurl, but instead two “knurl”
ribs similar to a double thread are formed on the periphery. This
construction makes it possible to sink the knurl into the work to the
proper depth without exerting excessive pressure on the arbor and
throwing it out of line.
[Illustration: Fig. 22. Three-inch Shrapnel Shell made on a Gridley
Automatic Turret Lathe]
=Second Series of Operations on “Frankford” Forged Shrapnel
Shell.=--For the second series of operations, the “Frankford” shrapnel
shell is held in a draw-in collet as shown in Fig. 21. As the shell
has been completely machined on the outside, it is let into the collet
for a considerable distance. For machining, it is shown gripped in
the collet by jaws _A_ and is backed up by positive stop _B_. At the
first turret face, tool _C_ rough-bores the diaphragm seat, tool _D_
bores the thread diameter, and tool _E_ faces and chamfers the end.
The turret is now indexed, and tools _F_, _G_, and _H_ perform similar
finishing cuts. A holder held on the third turret face carries tool
_I_ that chamfers the powder pocket, and at the fourth turret face a
collapsible tap threads the open end.
[Illustration: Fig. 23. Tool set up for Producing the Shell shown in
Fig. 22]
=Making Shrapnel Shells on the Gridley Automatic Turret Lathe.=--Figs.
22 to 25 show a three-inch shrapnel shell made on the 3¹⁄₄-inch Gridley
single-spindle automatic turret lathe. The steel from which the shell
is made is very tough. The specifications are from 125,000 to 135,000
pounds tensile strength, 110,000 pounds elastic limit, a twenty-five
per cent reduction of area, and a twelve per cent elongation. It will
be seen from the above specifications that the steel is, of necessity,
very tough and difficult to work; in addition, a large taper reamer
must be used, and the outside of the shell must be relieved throughout
the central portion. It is also necessary to machine the piece to
extremely accurate dimensions, all of which tends to make the work
still more difficult. Fig. 22 shows a view of the shrapnel shell.
It is approximately three inches in diameter and eight inches long,
and the limits allowed for the sizes are extremely close throughout,
both inside and outside. Figs. 24 and 25 show the successive steps
employed in machining the piece complete, the four views presented
representing the appearance of the work and the operations performed at
each indexing of the turret. Fig. 23 will enable the operation of the
different parts to be more clearly understood.
[Illustration: Fig. 24. Successive Steps and Operations employed in
Making the Shell shown in Fig. 22]
[Illustration: Fig. 25. Successive Steps and Operations employed in
Making the Shell shown in Fig. 22]
While the operation of the Gridley automatic turret lathe is generally
understood by mechanics, it may be well to state briefly the general
principles upon which work is done in the single-spindle machine. In
this type of machine, the position of the work does not change as it
does in the multiple-spindle machine, but the turning is accomplished
by the operation of tools mounted on tool-slides which, in turn,
work on a turret that revolves about a horizontal axis, successively
presenting the tools for operation upon the work. This will be readily
understood by glancing at the illustration Fig. 23. It will also be
noticed from this illustration that the forming tools and cutting-off
tools are operated from a face-cam at the lower part of the machine.
The forming slide is actuated by a cam groove cut in one side of the
cam-plate while the cutting-off slide receives its movement from a cam
groove on the reverse side of this plate.
At the first position of the turret, a large 2¹¹⁄₃₂ inch high-speed oil
drill is run into the bar to a depth of 6¹⁄₃₂ inches, and, at the same
time, a knee-turner located on the tool-slide turns the outside of the
stock, thereby removing the scale from the bar. Referring to Fig. 23,
which shows the turret in the third position, the end of this large
drill is shown at _A_, and, of course, when at work, it would be in the
position of the reamer which is shown at _F_. The time elapsed at the
completion of this part of the work is eleven minutes, five seconds.
[Illustration: Fig. 26. First Chucking on Warner & Swasey Turret Lathe
for machining British Forged Shrapnel Shells]
At the second position of the turret, a smaller drill, 2¹⁄₁₆ inches
in diameter, which is shown at _B_, is run in at the bottom of the
hole previously drilled to a depth of ²⁹⁄₃₂ inch. At the same time a
counterboring tool, which is located at _C_ and which is attached to
the drill with a set-screw, is at work counterboring the end of the
hole in the shell. During the time that this drilling and counterboring
operation is being performed, the forming tool shown at _D_ is being
fed into the outside of the head of the shell, finishing the three
grooves as shown; in addition, a sizing tool _E_, which is at a fixed
distance from the forming tool, comes in and sizes the work to exactly
the right length. The time elapsed up to the finishing of this part of
the work is thirteen minutes, thirty-five seconds.
[Illustration: Fig. 27. Diagram Illustrating Position and Relation of
Tools for First Chucking on British Forged Shell]
At the third position of the turret, which, by the way, is the one
shown in Fig. 23, the large taper reamer _F_ is run in, which operation
removes the bulk of the stock for the taper, and a second step at the
end of this reamer finishes the extreme end of the hole at the bottom
of the shell. The blades of this reamer are nicked to break the chips
as they are being formed. Before the reamer begins to cut, the knurling
tool _H_ is brought against the work (while it is on the high speed)
by the cutting-off slide, which, of course, results in a better knurled
section than would result if the knurling of the piece were done at a
lower speed. During the reaming operation, the cutting-off tool _G_
is run in part way to facilitate the final severing of the piece. In
addition, the relieved part of the work is turned by a tool mounted in
a tool-holder on the slide of the turret. This tool is shown at _I_
and it is operated by a templet _J_ which has a raised projection that
throws the tool into the work after it has reached the right position
with relation to the length of the shell. The total time elapsed up
to the finishing of this part of the work is twenty-two minutes,
thirty-five seconds. At the fourth and last position of the turret, a
finishing reamer sizes the outer end of the interior of the shell and
is withdrawn but part way, so that, when the cutting-off slide comes in
and finishes severing the piece, the shell is caught on the reamer and
not allowed to drop and possibly be injured by so doing.
[Illustration: Fig. 28. Set-up on Warner & Swasey Turret Lathe for
Second Series of Operations on Forged Shrapnel Shell]
The average total time for making this piece complete is twenty-seven
minutes. On account of the rigidity of the tool support, the tools do
not require sharpening more often than once for fifty pieces, with the
possible exception of the cutting-off tool, which must be sharpened
after about half that number of pieces have been completed.
=Using Warner & Swasey Turret Lathe for Machining Forged Shrapnel
Shells.=--In Fig. 26 is shown a typical set-up on a Warner & Swasey
No. 2A universal hollow-hexagon turret lathe for machining an 18-pound
shrapnel shell forging. The arrangement of the various tools for
performing the first series of operations is more clearly illustrated
in Fig. 27, to which reference should now be made. The forging is
located for machining on a special arbor fitted into the spindle and
carrying two spring-controlled centering bushings _A_. These serve to
locate the shell, which is then gripped by the floating jaws of the
chuck on the external diameter, and a stop on the end of the arbor
locates the shell from the bottom of the powder pocket.
[Illustration: Fig. 29. Diagram Illustrating Sequence of Operations
performed at Second Chucking]
The first operation consists in taking a cut from the external
diameter with a special box-turner provided with a roll steadyrest
and carrying two turning tools. The second operation is handled from
the cross-slide, the shell forging meanwhile being supported by a
roll steadyrest clamped to the turret. In this operation the closed
end of the shell is faced with tool _C_, the corner rounded, and the
band groove formed with forming tool _D_. The third operation--first
chucking--is performed with tool _F_ which produces the waves in the
band groove, and is operated in the following manner: Referring to the
lower left-hand corner of the illustration, it will be seen that a
roll _G_ is brought in contact with the face-cam _B_, thus giving the
desired oscillating movement to the waving cutter. The fourth and final
operation consists in under-cutting the band groove with a tool clamped
to the turret. This tool gages from the end of the shell by a revolving
stop _H_, and is provided with two slides, set at the desired angle
to each other and the work, carrying under-cutting tools _I_ and _J_.
These slides are operated by handle _K_.
[Illustration: Fig. 30. Third Chucking Set-up on British Forged
Shrapnel Shell]
The second chucking on this shell is handled as shown in Figs. 28 and
29 on the same type of machine. As shown in Fig. 29, the shell for
this operation is gripped in an automatic chuck, and a stop _A_ for
locating it is held in the spindle. The first operation consists in
roughing out the powder pocket and diaphragm seat with a cutter _B_,
and rough-turning that portion of the shell held in the chuck in the
previous chucking with a tool _C_. This tool is held in the cross-slide
toolpost, and is controlled in its movement by a special guide fastened
to the regular taper-turning attachment. The second operation finishes
the powder pocket and diaphragm seat with a cutter _D_.
[Illustration: Fig. 31. Diagram Illustrating Relation of Tools for
performing Third Series of Operations]
[Illustration: Fig. 32. First Chucking on French Shell made from Bar
Stock on Warner & Swasey Turret Lathe]
After the second chucking, the shell is heated on the nose, closed
in and is then brought back to the turret lathe, when the operations
are performed as shown in Figs. 30 and 31. Here, again, the forging
is held in the automatic chuck and is located by a plug _A_ in the
spindle. The first series of operations consists in boring, facing
and chamfering the nose with a counterbore _B_, and at the same time
turning the external radius on the nose with a tool _C_. Tool _C_ is
held in the cross-slide square turret and is controlled in its movement
by a special guide fitting on the regular taper-turning attachment.
The second operation, shown to the left of the illustration, consists
in machining the radius inside the nose with a tool _E_, controlled
in its movement by the special guide _D_, as previously mentioned.
The third and final operation consists in cutting the thread with a
collapsible tap _F_.
[Illustration: Fig. 33. Second Chucking on French Shrapnel Shell]
=Using Warner & Swasey Turret Lathe for Machining Bar-stock Shrapnel
Shells.=--The method of machining shrapnel shells from bar stock
differs somewhat from that used for forgings, and is handled on a
No. 2A universal hollow-hexagon turret lathe. In this particular
case, the shell blank, previous to machining in the turret lathe, is
rough-drilled in a high-powered drilling machine to the bottom of the
powder pocket. Assuming that this has been accomplished, the operations
for the first chucking are then carried on as illustrated in Fig. 32.
Here the shell is held in an automatic chuck and is located by a stop
_A_. The first operation consists in counterboring the mouth with the
counterbore _B_, and rough-turning the external diameter with tool _C_;
second, counterboring with the cutter _D_ and turning further along the
shell with a tool _E_; third, finishing the bottom with a cutter _F_
and facing the end of the shell with a tool _G_.
[Illustration: Fig. 34. Third and Final Chucking on French Shrapnel
Shell]
In the second chucking, the operations shown in Fig. 33 are performed.
Here the shell is reversed in the automatic chuck and is located, as
before, by a stop _A_. The first operation consists in turning that
portion of the body held in the chuck in the previous chucking with a
roll-supporting turning tool _B_. Second, supporting the shell with a
roller support _C_ held on the turret, facing the end with a tool _D_,
and chamfering the band groove and the end with a cutter _E_ held on
the cross-slide square turret. The third operation is to support the
shell from the turret, knurling with a knurl _F_ from the cross-slide
square turret. Fourth, taper-turn from the end to the band groove with
a tool _G_, guided by the taper-turning attachment.
For the third chucking, the shell, as indicated in Fig. 34, is held in
the same manner as for the first chucking. First, it is recessed with
a tool _A_ and brought into action by operating the special holder
which has a cross-sliding movement; second, it is bored and faced
with a counterbore _B_ from the turret, and taper-turned with a tool
_C_ operated by a special guide from the taper-turning attachment. In
the third operation, the thread in the nose is rough-chased with a
tool _D_, controlled in its movement by the chasing attachment of the
machine; fourth, the thread is finished with a tap and tap-holder _E_.
[Illustration: Fig. 35. Diagram showing Method of holding and
performing First Series of Operations on Forged Shells on “Lo-swing”
Lathe]
=Machining Shrapnel Shell Forgings on the “Lo-swing” Lathe.=--By adding
a simple carriage to its “Lo-swing” lathe, the Fitchburg Machine Works,
Fitchburg, Mass., has adapted this machine for machining shrapnel
shells of different types. The following data and illustrations refer
particularly to tooling used for machining the Russian and French
shells. On the Russian shell, after centering, the forging _A_ is held
on a special arbor _B_ shown in Figs. 35 and 36. Placed over this arbor
is an expanding collar _C_, the inside surface of which is chamfered to
fit against surface _D_ on the stem of the arbor. The section of the
arbor next to the spindle is threaded and a large nut and handwheel
_E_ are turned to pull the sliding sleeve _C_ along the arbor and thus
expand it to firmly grip the inside of the shell forging. Sleeve _C_ is
connected to the nut _E_ by a threaded collar _F_. After the forging is
securely located on the arbor, which it should be understood extends to
the bottom of the powder pocket to gage it for length, the tail-center
_G_ is run in to support it.
[Illustration: Fig. 36. Set-up for performing First Series of
Operations on Russian Forged Shell on “Lo-swing” Lathe]
To those familiar with the “Lo-swing” lathe, it will be appreciated
that its chief efficiency lies in its system of multiple turning
tools. Thus, on this job, tools _H_, _I_, _J_, _K_, _L_, and _M_ are
all mounted on one slide, and in the illustration are shown in the
positions they occupy after taking their respective cuts. At the
beginning of the cut, turning tools _K_, _L_, and _M_ are drawn back
clear of the work to allow sufficient clearance for tools _H_ and _I_
to operate. With the tools drawn back and the carriage at the extreme
right of the bed, tool _H_ is the first to come in contact with the
work. This tool takes a roughing cut over the body of the forging,
finishing at the radius on the nose.
Tool _H_ is controlled in its action by a former pin on the tool-slide,
held in contact with the face of cam former _O_ by a stiff spring.
Former slide _O_ takes the place of the regular taper-turning former
ordinarily used on the “Lo-swing” lathe. When the former pin in the
slide carrying tool _H_ reaches point _P_ on former _O_, the tool is
withdrawn to conform with the shape shown at _N_ on the forging. The
tool is then fed in further toward the axis of the arbor, until the
former pin reaches point _Q_ on the slide, when the radius on the nose
is completed. Tool _H_ is the only one mounted on a taper-turning block.
[Illustration: Fig. 37. Diagram showing Method of performing Second
Series of Operations on Forged Shrapnel Shells on “Lo-swing” Lathe]
Just after tool _H_ passes point _N_, tool _I_ commences to cut at
the end of the forging, taking a finishing cut and ending up in the
position in which it is shown in the illustration. After tool _I_
reaches this position, the other tools _J_, _K_, _L_, and _M_ are
brought into action. Tools _K_, _L_, and _M_ are so situated on the
carriage that no lateral feeding is required. When these tools are in
action, the roller support _R_ takes the thrust. Tool _K_ roughs out
the band groove and is fed into the work by a handwheel. Tool _L_ cuts
the groove for attaching the brass case to the shell, and tool _M_,
carried on the same block, faces the end. Tools _K_, _L_, _M_, and _S_
are located on the same carriage and are fed in together. Tool _S_
rounds the corner of the shell. The carriage on which tools _K_, _L_,
_M_, and _S_ are located is now drawn back out of the way, and the
entire carriage moved over so that tool _J_ can be used to under-cut
the rifling band groove. After cutting off the center projection, the
first series of operations on the shell is completed.
[Illustration: Fig. 38. Set-up on “Lo-swing” Lathe for performing
Second Series of Operations on Russian Shell]
=Second Series of Operations on the Russian Shell.=--The second series
of operations is performed on the inside of the shell on the “Lo-swing”
lathe, which is provided with a special turret for this purpose. As
is shown in Figs. 37 and 38, the shell _A_ is held in special collet
jaws _B_ that have a two-point bearing on the shell. Stop _C_ in the
spindle locates the shell in the chuck. To manipulate the chuck for
tightening it on the work, handwheel _D_ is turned, carrying with it
the nut _E_ and ring _F_. Ring _F_ carries pins sliding in slots in
sleeve _H_ and driven into collet _B_, so that when nut _E_ is drawn
back it also carries collet _B_ into the taper in sleeve _H_, closing
the collet on the work. Turning handwheel _D_ in the opposite direction
releases the grip of the collet _B_ on the work. The first operation is
performed with tools _I_, _J_, _K_, and _L_. Tool _I_ bores the powder
pocket, tool _J_ roughs the diaphragm seat, tool _K_ rough-turns the
thread diameter at the shell mouth, and tool _L_ faces the end. The
turret is now indexed, and boring-bar carrying tool _M_ is brought
into operation. This tool turns the curved interior of the shell. To
accomplish this, the turret locking-pin is removed, allowing the turret
to float on its central axis. Fastened on the ways of the lathe at the
rear of the turret by a clamp _O_ is the cam bracket _N_ carrying the
guiding cam _P_. This cam, through pins _Q_ and _R_ in bracket _S_,
controls the float of the turret and guides the cutting tool _M_. In
the illustration, the tool is shown at the end of the cut. It will
also be noted that one surface of the cam is curved and the other is
straight; therefore, to compensate for this and also to steady the
turret, pin _R_ is backed up by a spring. Clamp _O_ is now released and
bracket _N_ moved back to allow the turret to be indexed. Bracket _N_
is located, when brought into the operating position, by a stop on the
bed of the lathe.
[Illustration: Fig. 39. Diagram showing Method of machining French
Shells on “Lo-swing” Lathe--First Series of Operations]
[Illustration: Fig. 40. Diagram showing Method of holding and applying
Tools on “Lo-swing” Lathe for performing Second Series of Operations on
French Shell]
In the third position, tool _R_ finishes the powder pocket, _S_ the
diaphragm seat, and _T_ the thread diameter, whereas _U_ acts as an
adjustable stop for the depth of the various tools. The fourth and last
operation is tapping with a collapsible tap _V_. This completes the
machining of the Russian shell on the “Lo-swing” lathe.
=Machining French Shrapnel Shell on “Lo-swing” Lathe.=--The machining
of the French shrapnel shell is well suited to the “Lo-swing” lathe.
A great many of the French shells are made from solid bar stock, and
when this is the case, the first operation, performed as shown in Fig.
39, consists in rough-drilling. If the shell is made from a forging,
this operation, of course, is dispensed with and the first tool used
carries boring and facing cutters, as shown at _A_, _B_, _C_, and _D_.
These rough-bore the three diameters on the inside of the shell and
face off the end to length. The next operation is accomplished with
two finishing boring tools _E_ and _F_, the depth of which is obtained
by an adjustable collar _G_ that comes against the produced with a
collapsible tap _H_. The turret is then indexed two holes, bringing the
special recessing tool into position. This tool is of the cross-slide
type and carries a back recessing cutter _I_. This completes the first
series of operations on the shell.
[Illustration: Fig. 41. Set-up on “Lo-swing” Lathe for performing
Second Series of Operations on Straight Type of French Shell]
=Second Series of Operations on Shell. French=--The second series of
operations on a French shell is accomplished as shown in Fig. 40. Here
the shell is held in the same manner as described in connection with
Fig. 35. The forging is placed on arbor _B_ that has an expanding
sleeve _C_ operated by the hand-clamping wheel nut _D_. Eight cutting
tools are located on the carriage. Tool _A_ turns the diameter at the
open end of the shell, _B_ the central part, _C_ cuts the band groove,
_D_ chamfers the section adjacent to the band groove, _E_ chamfers
the end of the shell, and _F_ knurls the band groove. Roll _G_, in
connection with roll _H_, supports the shell while the knurling is
being done, whereas tool _I_ faces off the end of the shell. At the
beginning of the cuts, tools _C_, _D_, _E_, and knurl _F_, also roll
_G_ and tool _I_, are withdrawn. This permits tool _A_ to cut the front
end of the shell at the beginning and finish the diameter at the open
end of the shell. Tool _B_ next comes into action and turns the central
part of the shell. Tool _C_ is then located in the correct position for
the band groove and the carriage on which tools _C_, _D_, and _E_ are
located is fed straight in, cutting the band groove and chamfering.
Knurl _F_ is then brought into position to knurl the groove, with roll
_G_ backing up the work against roll _H_. The last operation is to cut
off the center projection with tool _I_.
Fig. 41 shows the tool set-up on the “Lo-swing” lathe for machining
the straight type of French shell, in which two tool-blocks are used
for doing the straight turning. The leading tool turns the end of the
shell a little larger than the main body. The procedure for grooving,
knurling, and facing the shell is that previously described for the
forged shell, which is shown in Fig. 35. On the French shrapnel shell
the second operation follows directly after the first, whereas on
the Russian forged shell a nosing-in operation comes between the two
machining operations.
[Illustration: Figs. 42 and 43. Set-up and Tool Equipment on the
“Libby” Turret Lathe]
=Using the “Libby” Turret Lathe for Machining Shrapnel Shells.=--One of
the many ways of machining a shrapnel shell is illustrated in Figs. 42
and 43. This shows the set-up on the “Libby” turret lathe, manufactured
by the International Machine Tool Co., Indianapolis, Ind. In the first
chucking, the forging, as shown at _A_, is held on a special solid
arbor provided with a series of corrugations where it contacts with
the forging. This, in addition to providing a rigid support, assists
in gripping, and the shell is also gripped by a pair of chuck jaws
that act as drivers. First, a gang tool-holder carrying three stellite
turning tools _o_ is brought into position, and the cutting is
started, continuing for a distance of one-third of the length turned.
To provide additional support, a roller back-rest, carrying a facing
tool, is brought in to steady the work, and, as it is fed forward, the
end of the forging is faced off and chamfered.
[Illustration: Figs. 44. and 45. Machining Shrapnel Shell Forgings on a
22-inch Extra-heavy Turret Lathe]
The second operation on the first chucking is shown at _B_. Here the
cutter _a_ is brought in first and starts the band groove, after which
the under-cutting tool _b_ is brought in to under-cut the edges of
the groove. In the meantime, roller _c_ supports the work. Upon the
completion of the groove, the holder carrying cutter _d_ is advanced to
finish-face the end of the work and chamfer.
The third operation--cutting the waves in the band groove--is of an
interesting character and is accomplished as shown at _C_. A cam _e_
which is free to rotate with the work is first brought in contact with
it; then the cross-slide is advanced, carrying the waving tool _f_ and
the guide _g_. The guide _g_ fits in the cam groove and controls the
operation of the waving tool.
In the second chucking on the first operation the shell is reversed
in the chuck and is held in the manner indicated at _D_, Fig. 43. The
forging is located in the chuck by a stop-collar _h_, and is gripped on
the external diameter by the jaws of the chuck. A stepped boring tool
carrying five inserted blades is brought in to rough-bore the internal
diameters and machine the shell to the proper thickness at the bottom
of the powder pocket. This tool also carries a facing cutter that faces
off the shell to the proper length. While the boring tool is working,
a broad turning tool, held on the cross-slide, is brought in to bevel
the nose preparatory to closing-in. The next step is to taper-ream the
internal diameter, as shown at _E_. This completes the operations for
the second chucking.
The nose of the shell is now heated and closed in, after which the
third series of operations is performed. The first step in the third
chucking is to bore for the thread and face the end of the shell with
a turret tool, as shown at _F_. The next operation is to machine the
curved contour of the nose of the shell with a special turret tool
as shown at _G_. Here a wide forming cutter _i_, held in a turret
tool-holder, is brought in contact with the work, finishing the nose
of the shell to the proper form. During this operation, the shell is
supported by a roller in the holder.
The next operation is to form the inside of the nose of the shell to
the proper shape, as shown at _H_. This is accomplished with a forming
blade _j_, held in a holder clamped in the toolpost. Following this, a
collapsible tap is brought in from the turret to thread the nose of the
shell, as shown at _I_.
[Illustration: Fig. 46. Method of holding Shrapnel Shells for First
Operation on a 22-inch Turret Lathe]
=Machining Shrapnel Shells on a Heavy 22-inch Turret Lathe.=--Still
another method of machining shrapnel shells in a heavy turret lathe
is shown in Figs. 44 and 45. The shell being machined is an 18-pound
British shrapnel shell made from a forging. It is held on an expanding
arbor for the first operation, as shown in Fig. 46. The arbor is of
the three-point support type and is positive in its grip. Around the
periphery of the nose-piece are located three pinions _A_ capable of
being rotated by a square-ended wrench. These mesh with teeth in bevel
gear _B_ which, in turn, is threaded onto arbor _C_. The forward end of
this arbor is cone-shaped and operates the three gripping fingers in
the open end of the shell, whereas another rod passing through arbor
_C_ and connected to plunger _D_ operates, through the coil spring, the
three fingers used in gripping the shell by the powder pocket. This
arbor holds the shell securely while the machining operations are being
accomplished.
The first operation performed at the first chucking of the work is
shown at _C_ in Fig. 44. Here a turning tool-holder clamped to the
turret and carrying two cutters is advanced and takes a roughing cut
from the exterior diameter of the shell for practically its entire
length. The shell is supported by three roller supports as illustrated.
The second operation at the first chucking is performed from the
cross-slide, as shown at _D_. Here a forming tool of the tangent type
roughs out the rifling band groove, leaving sufficient metal in the
center for the production of the wave ribs. The third operation is
facing off the closed end of the shell from the turret as shown at
_E_, and the fourth operation consists in machining the waved ribs as
shown at _F_. The tool for accomplishing this operation is held on the
cross-slide and is operated from a face-cam on the nose of the spindle.
[Illustration: Fig. 47. Cutting Square Thread in Nose of French
Shrapnel Shell In “Automatic” Threading Lathe]
In the second chucking the shell is held in a three-jaw scroll chuck.
The first operation is to rough-bore the inside of the shell and powder
pocket with a tool _G_, Fig. 45, held in the turret; directly after
this a finishing tool of the same shape is brought in, finishing the
surfaces previously roughed out. The second operation is to face off
the open end of the shell and taper-form back of the nose from the
cross-slide, as shown at _H_, and at the same time turn that portion
of the exterior surface of the shell not machined in the previous
operation with a tool clamped to the turret as shown at _I_.
[Illustration: Fig. 48. Threading Base End of Bar-stock Shrapnel Shells
in “Automatic” Threading Lathe]
Previous to the third chucking, the nose of the shell is heated and
closed in. The shell is then held in a three-jaw scroll chuck provided
with special jaws. The first operation, as shown at _J_, consists
in boring and turning the nose of the shell with a tool held in the
turret. Following this, the hole is reamed with a standard reamer and
tapped with a collapsible tap. Both of these tools are held in the
turret, but are not shown in the illustration. This completes the
machining operations on the shell.
=Threading Shrapnel Shells on “Automatic” Threading
Lathes.=--Considerable difficulty has been experienced in cutting the
square thread in the nose of the French shrapnel shell. One method
which accomplishes this operation satisfactorily is shown in Fig. 47,
and is accomplished on a 12-inch “Automatic” threading lathe built by
the Automatic Machine Co., Bridgeport, Conn., and equipped with special
tools for this purpose. Referring to this illustration, it will be seen
that two tools are used--a roughing tool _A_, and a finishing tool _B_.
Tool _A_ roughs out the thread to a shape similar to the Acme type of
thread, whereas tool _B_ squares it up. The roughing and finishing
tools are held on the forward and rear carriages, respectively, and
are operated simultaneously, being advanced throughout the length of
the thread, withdrawn and returned to start a new cut. The method of
operating the tools is one of the chief features of the “Automatic”
threading lathe.
[Illustration: Fig. 49. Turning, facing, and threading Plugs for Closed
End of Bar-stock Shrapnel Shells in “Automatic” Threading Lathe]
The base end of shrapnel shells when made from bar stock is as a rule
bored out and a plug inserted to eliminate any piping effect in the
bar. Fig. 48 shows the method of accomplishing this operation on a
12-inch “Automatic” threading lathe. The work is held in a three-jaw
universal chuck and is supported by a roll steadyrest comprising two
rolls that are located beneath the work. On the extended end of the
rear roller stud is fastened a swinging stop that is used for locating
the base of the shell in the correct position ready for threading. The
base of the shell is counterbored in another machine, previous to the
threading operation. The threading is done with a circular tool held
on a special internal threading tool-holder, the latter being retained
in the toolpost carriage. The threading tool-holder can be moved
longitudinally to bring it into the proper relation to the work. It is
also held so that the cutting edge is turned upside down as this action
forces the work down in contact with the roller supports. By handling
the work in this manner, a steadyrest of the ordinary type is dispensed
with and the operation of the attachment facilitated.
[Illustration: Fig. 50. Grinding Shrapnel Shells on a Norton
Special-purpose Grinding Machine]
One method of making plugs for the base end of shrapnel shells when
made from bar stock is shown in Fig. 49. For this work, a 12 by 4
“Automatic” threading lathe equipped with special tools designed for
this purpose is used. The machine is provided with a draw-in collet
chuck that holds the rough-forged blank. The order of handling the
operations on this machine is to use the rear tool _A_ for turning
the external diameter of the plug. This is handled at the same rate of
feed as that required for threading, so that it is sometimes necessary
to take more than one cut, depending on the amount of material left on
the diameter. The vertical slide _B_ is for facing only and carries a
cutting tool _C_. This is supposed to finish the face in one cut, but
as the work will spring considerably, a light finishing cut is taken
when the tool is being drawn back from the center to the circumference
of the work. The threading tool _D_ is held on the front toolpost
and is of single-point construction. The feed given to this tool is
automatically controlled, both as to pitch and depth of cut at each
traverse.
[Illustration: Fig. 51. Diagram showing Scleroscope Hardness Test of
Heat-treated Shrapnel Shell at Various Points along its Surface]
In actual operation, both the threading and turning tools are in motion
all the time on the work, but the tools are independently controlled
so that either one can be operated separately. A stop is provided on
the back toolpost so as to turn each plug to the same diameter. The
automatic throw-out for the feed of the threading tool is set from the
front handle on the ratchet and pawl as regularly furnished on the
“Automatic” threading lathes.
=Grinding Shrapnel Shells.=--An increasingly large number of shrapnel
shell manufacturers are finishing the steel shell by grinding instead
of finish-turning. That is, the exterior surface of the shell is
rough-turned to within from 0.030 to 0.080 inch of the finished size
and is then finished to the required limits and shape by grinding,
as shown in Fig. 50. It is claimed by the advocates of grinding that
the finishing operations are more speedily performed in this manner
and that a more accurate and concentric shell is produced. They also
point out the fact that portions of the shell are so hard that it is
extremely difficult, if not impossible, to turn it in the allowable
time.
The varied heat-treatment given to the shell on the closed end and nose
leaves it harder in some sections than others, as indicated in Fig.
51. The section _E_, 2¹⁄₂ inches from the closed end of the shell,
must strike from 42 to 50 on the scleroscope, and the section _A_ at
the nose must strike between 20 and 25. The section marked _D_, or
that part of it to the left of the line that marks the limit of the
heat-treating on the closed end, has not been heat-treated at all, and
partly on this account, and also because of the gradually diminishing
thickness of the shell along this section, it strikes between 40 and
45, decreasing as the thickness of the wall diminishes, until at _C_
the section strikes but 35. Section _B_, adjacent to the annealed nose
of the shell, strikes about 30 on the scleroscope.
[Illustration: Fig. 52. Two-operation Method of grinding Shrapnel
Shells on Norton Grinding Machines]
On the other hand, some manufacturers are not putting the shell through
this heat-treating and tempering process, and omit the annealing and
machining of the nose after the nosing-in operation. This leaves the
nose with considerable stock to remove and in such a condition as
regards hardness that the grinding machine becomes a necessity. In
the face of these varying degrees of hardness of the shrapnel shell,
it will be seen that it is difficult to secure wheels of the right
grain and grade to suit all of these conditions. With this information
in mind, we can more intelligently take up the actual grinding of the
shell. The Norton Grinding Co., Worcester, Mass., has been actively
engaged in developing methods of grinding shrapnel shells and the
following illustrations and descriptions apply to this work.
[Illustration: Fig. 53. Three-operation Method of grinding Shrapnel
Shells on Norton Grinding Machines]
Fig. 52 shows the two-operation method of grinding the shrapnel shell.
Section _A_ at the open end of the shell is covered by a wide-faced
wheel formed to shape, that finishes the radius on the nose at one
in-feeding of the wheel. Sections _B_, _C_, and _D_ are covered by a
wide-faced wheel, formed to shape so as to finish these three surfaces
at one in-feeding of the wheel. Section _E_ at the closed end of the
shell is finished completely by turning.
Some manufacturers use a three-operation method of grinding the
shrapnel shell as illustrated in Fig. 53. In this case, the sections
_A_ and _D_ are first ground with the same wheel, as American
manufacturers deem it advisable to grind surface _A_ rather than
to finish it by turning. The second stage in this grinding is the
finishing of the nose _E_ with a formed wheel, and the third stage is
the finish-grinding of the body at points _B_ and _C_.
=Two-operation Method of Grinding Shrapnel Shells.=--The procedure
followed in grinding shrapnel shells by the two-operation method is
first to screw plugs into the open end of the shells, as shown in Fig.
52. The outer ends of these plugs are centered, and the projection
left on the closed end of the shell with the center intact acts as a
means of supporting the shell. Some of the Canadian manufacturers vary
this practice by cutting off the center projection on the closed end
of the shell and fitting a cap with a center hole over the closed end.
Others use a ball-bearing cup center to carry the closed end. American
manufacturers, however, leave the center projection on the shell until
after the grinding has been finished.
[Illustration: Fig. 54. Radius Wheel-truing Device for forming Grinding
Wheel for grinding Shrapnel Shell Nose]
In grinding the nose end of the shell, the amount of metal removed
varies from 0.020 to 0.090 inch on the diameter. The grinding wheel
operates at from 6000 to 6250 surface feet per minute. The speed of the
work is 75 revolutions per minute, or a surface speed of practically
75 feet, and the machine used is a Norton 6 by 32 plain grinder. The
wheel used is generally 14 inches in diameter by 2¹⁄₄-inch face. The
wheel requires truing for every five to twenty shells, depending upon
the amount of metal removed and the hardness of the shell. For truing,
a simple radius fixture carrying a diamond is used. Fig. 54 shows this
wheel-truing device clamped on the grinding machine bed. It is applied
in the same manner as the usual steadyrests used for supporting the
work. The diamond is mounted in a swinging arm that is operated by a
hand lever as shown. By successive cuts across the wheel, the desired
shape is attained.
[Illustration: Fig. 55. Norton Special Form Wheel-truing Device for
truing Wheel for grinding Shrapnel Shell Body]
For grinding the body either a 10 by 24 special-purpose or 10 by 36
Norton grinding machine is employed. The amount of metal removed
from the body varies from 0.030 to 0.075 inch on the diameter, and
the limits vary from 0.002 to 0.010 inch, depending largely on the
requirements of the plant in which the work is being done. The wheel
used on the body is 20 inches in diameter and is of the ring-wheel
type. It will be noticed in Fig. 52 that the wheel for grinding the
body is also formed to shape. The method of truing the wheel for
shaping the shrapnel shell body is shown in Fig. 55. This attachment
is clamped to the front of the grinding machine bed and at the top of
the bracket is fitted a slide _A_ operated by handwheel _B_. Upon the
face of this slide nearest the grinding wheel is pivoted an angular
arm _C_ that supports the diamond _D_ at its lower end. Under the end
of the upper arm is a spiral spring that keeps the diamond normally
back from the wheel. A plate former _E_ clamped to the bottom face of
the bracket is shaped to agree with the form to be given the wheel. At
the lower extremity of the arm and behind the diamond is mounted a roll
_F_ that bears constantly against form _E_. When the diamond slide is
reciprocated by turning the handwheel, the diamond is made to traverse
a path conforming with the cam that guides it. By moving the wheel in
toward the diamond and making successive traversings of the diamond,
the wheel is given the desired shape.
[Illustration: Fig. 56. Besly No. 14 Ring Wheel Grinder equipped for
grinding Shrapnel, but shown without Hoods and Water Attachments]
[Illustration: Fig. 57. Fixture used on Besly No. 14 Ring Wheel Grinder
for grinding Center End from Shrapnel Forgings]
For grinding the body, the wheel must be trued after every ten to
twenty-five shells are ground, depending upon the amount of metal
removed and the hardness of the shell. In grinding shrapnel shells, the
usual method is to fit a lot of the shells with the driving plugs and
carry them all through to completion before removing the plugs.
=Removing Center End From Shrapnel Forgings.=--For performing
practically all the machining operations on the shell, a center
projection is left on the closed end of the shell for supporting it.
This, of course, must be removed before the shell is completed. One
method of doing this is to use a Besly No. 14 ring-wheel grinder
equipped with a special fixture. A Besly grinder fitted up for this
work is shown in Fig. 56, and the fixture used for holding the shell
is shown in Fig. 57. The machine, as furnished, is arranged for wet
grinding, but is not so fitted up in the illustration. The fixture
is fastened to the geared lever feed table and is of simple design.
It is provided with a backing-up stop _A_, the work resting in two
semi-spherical groove projections on the fixture. The operator simply
holds the shrapnel shell in place by hand and then feeds it in against
the wheel and traverses it past in the usual manner. The time for
removing a ⁵⁄₈-inch diameter stub end projecting ³⁄₈ inch from the body
of the shell is less than a minute.
[Illustration: Fig. 58. Tools for making Base of Powder Cup]
[Illustration: Fig. 59. Tools for making Top Member of Powder Cup]
=Press Tools for Making Powder Cup.=--In the British shrapnel shell,
the powder in the base of the shell used for exploding it and ejecting
the lead bullets, etc., is held in a tin-plate powder cup. This is
completed in the punch press in the manner shown in Figs. 58 and 59,
and comprises two parts, a base and a top. The base is made from tin
plate 0.022 inch thick, whereas the top is made from 0.036 inch thick
tin plate. The bottom of the cup is completed in one operation with
the punch and die shown in Fig. 58, which is held in a single-action
press. It is turned out from a blank 3⁷⁄₃₂ inches in diameter and is
cut out and formed in one operation. The completed size is 2¹⁄₄ inches
diameter by ⁷⁄₈ inch high. After cupping, the top edge is trimmed in
a turret lathe. The press operations on the top, as shown in Fig. 59,
are a little more complex. The first operation consists in cutting
out a blank 2¹⁹⁄₃₂ inches in diameter. Then the edge is turned up with
another punch and die shown in the center of the illustration. The next
operation is piercing the center with the punch and die at the right,
and the last operation is drawing out a flange around the pierced hole.
The tools for this operation are shown to the extreme right, as is also
a completed powder cup. The final operation on the cup consists in
soldering the top to the base.
[Illustration: Fig. 60. Diagram illustrating “Twelve-punch” Method of
making Shrapnel Bullets from Lead Wire]
=Shrapnel Bullets.=--The most deadly and effective parts of a shrapnel
are the lead bullets which are held in the shell. When the timing fuse
explodes the powder in the base of the shell, the nose is blown off
and the bullets are thrown out in a cone shape. The range covered by
these bullets in the 18-pound shrapnel shell is about 250 square yards.
The lead bullets, which in most shrapnel are ¹⁄₂ inch in diameter, are
made from several different compositions, but consist chiefly of 87¹⁄₂
parts lead and 12¹⁄₂ parts antimony. The number of bullets carried in
shrapnel shells of the different governments varies. There are 252 in
the American 15-pound shell, and 235 or 236 in the British 15-pound
shell. The bullets used by the U. S. government have six flattened
sides, to facilitate packing, whereas those used by foreign governments
are spherical.
There are several methods of making shrapnel bullets. One is to cast
the bullets in iron molds, which are split in the center, so that the
bullet can be removed when cast. Another is to cut off slugs from lead
wire and strike these between dies in a heading machine. The bullet
heading machine takes the wire from a reel, cuts it off, forms it and
trims off the resultant flash automatically. In making the American
bullets, a second operation follows, consisting in flattening the
sides. The Waterbury Farrel Foundry & Machine Co. furnishes unit
equipments for doing this work. For the flattened bullets, the unit
consists of one hydraulic wire extruding press and fourteen heading
machines capable of giving a production of 850 bullets per minute. For
the spherical bullet, the unit equipment consists of one hydraulic
extruding press and eight heading machines, giving a production of 950
bullets per minute.
The method of casting lead bullets in ordinary molds is antiquated, and
another method somewhat similar to that just described has taken its
place. The first step is to produce the wire from which the bullets are
eventually made. This is accomplished in two ways. The first is the hot
metal process and consists in pouring the molten lead into a cylinder,
from which it is extruded through a die by a plunger advanced into the
cylinder. By this method, it is necessary to allow the metal to settle
before the press can operate. An improvement over this is utilized in
presses built by a hydraulic lead press manufacturer of Brooklyn, and
consists in first casting ingots of the required diameter and length
and then charging the press with these instead of pouring the molten
lead into the press chamber. Two presses have been designed for this
process. One has a capacity of 700 tons and is charged with ingots
weighing 150 pounds, whereas the other has a 900-ton capacity and is
charged with 200-pound ingots. The product from these two machines is
1800 pounds of lead wire from the small and 2500 pounds from the large
press per hour. The wire as it is extruded from the die is wound on a
reel carrying 2000 pounds of wire.
There are two principal types of swaging machines used for making these
lead bullets from wire. One carries a single set of dies, whereas the
other carries twelve sets of tools. The operation of the latter will
be described. Referring to the diagram, Fig. 60, twelve reels of lead
wire--not shown--are arranged in tandem on stands behind the press, six
reels in a row. The wire is conveyed from these reels to the dies by
a feeding mechanism, being guided to the individual tools by a plate
_A_, having twelve U-shaped impressions in its top edge. The wire now
passes over a spring _B_ which serves to lift it up slightly at each
stroke of the press. The tools _C_ and _D_, as shown, are provided
with half-spherical depressions in their adjacent faces and are set so
that they come within ¹⁄₆₄ inch of meeting. The dies are guided and
controlled in action by a special mechanism, and the press in which
they are carried operates at 70 revolutions per minute. This gives a
rated production of 840 bullets per minute. As is clearly indicated in
the illustration, considerable scrap is formed in making lead bullets
by this process--in fact the scrap is about 33 per cent of the reel of
wire; also owing to the setting of the punches a slight fin is formed
around the periphery of the bullet.
After forming, the bullets are taken to a tumbling machine where
they are tumbled for one hour. No other material is put into the
tumbling barrel, but the action of the bullets working on themselves
satisfactorily removes all the fins. Both the swaging and tumbling
operations must be carefully watched because of the necessity of having
the bullets a certain weight. The allowable variation on one pound of
bullets is one dram, and there are forty-one bullets to the pound. Ten
pounds of lead rod make 6¹⁄₂ pounds of bullets, and the scrap resulting
from the swaging operation is remelted and used over again. After
tumbling, the bullets are inspected and are then ready for use.
CHAPTER V
MAKING FUSE PARTS
Combination timing and percussion fuses comprise a large number of
small parts made from different metals and alloys, and are produced in
various ways. Some of the parts are made from brass rod or alloys of
copper and aluminum, whereas others are made from hot-pressed forgings
and are machined after being formed to shape. In the following, a brief
description of several different methods of making the most important
fuse parts will be illustrated and described, together with details
regarding the forging tools used for the socket and plug.
[Illustration: Fig. 1. Tools used in forging Brass Fuse Socket]
[Illustration: Fig. 2. Diagram showing Construction of Tools used in
forging Fuse Socket]
=Forging the Fuse Socket.=--The fuse socket, which screws into the nose
of the shrapnel shell and acts as a base for the fuse, is made from a
special forgeable alloy casting containing 40 per cent copper, 58 per
cent zinc, and 2 per cent lead. The first step in this process is to
melt
Read full text (200,001 characters)
Fields
| author | Douglas T. Hamilton |
|---|---|
| language | English |
| chars | 459177 |
| source_url | https://www.gutenberg.org/ebooks/78213 |
Cite this record
MLA
"Shrapnel shell manufacture." Project Gutenberg, n.d., https://gutenberg.go-v.org/record/78213.
Chicago
"Shrapnel shell manufacture." Project Gutenberg. n.d.. https://gutenberg.go-v.org/record/78213.
APA
Project Gutenberg. (n.d.). Shrapnel shell manufacture. https://gutenberg.go-v.org/record/78213