Lead Smelting and Refining, With Some Notes on Lead Mining
The Project Gutenberg eBook of Lead Smelting and Refining, With Some Notes on Lead Mining This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Lead Smelting and Refining, With Some Notes on Lead Mining Editor: Walter Renton Ingalls Release date: November 16, 2020 [eBook #63784] Most recently updated: October 18, 2024 Language: English Other information and formats: www.gutenberg.org/ebooks/63784 Credits: Produced by deaurider, Les Galloway and the Online Distributed Proofreading Team at https://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) *** START OF THE PROJECT GUTENBERG EBOOK LEAD SMELTING AND REFINING, WITH SOME NOTES ON LEAD MINING *** Transcrib
The Project Gutenberg eBook of Lead Smelting and Refining, With Some Notes on Lead Mining
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: Lead Smelting and Refining, With Some Notes on Lead Mining
Editor: Walter Renton Ingalls
Release date: November 16, 2020 [eBook #63784]
Most recently updated: October 18, 2024
Language: English
Other information and formats: www.gutenberg.org/ebooks/63784
Credits: Produced by deaurider, Les Galloway and the Online
Distributed Proofreading Team at https://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)
*** START OF THE PROJECT GUTENBERG EBOOK LEAD SMELTING AND REFINING, WITH SOME NOTES ON LEAD MINING ***
Transcriber’s Notes
Obvious typographical errors have been silently corrected. Variations
in hyphenation other spelling and punctuation remains unchanged. In
particular the words height and hight are used about equally. As hight
is a legitimate spelling, it has not been changed.
Some of the larger tables have been re-organised to improve clarity and
avoid excessive width.
The footnotes are located at the end of the book.
Italics are represented thus _italic_.
LEAD SMELTING
AND
REFINING
WITH SOME NOTES ON LEAD MINING
EDITED BY
WALTER RENTON INGALLS
[Illustration: Publisher’s Device]
NEW YORK AND LONDON
THE ENGINEERING AND MINING JOURNAL
1906
COPYRIGHT, 1906,
BY THE ENGINEERING AND MINING JOURNAL.
ALSO ENTERED AT
STATIONERS’ HALL, LONDON, ENGLAND.
ALL RIGHTS RESERVED.
PREFACE
This book is a reprint of various articles pertaining especially to the
smelting and refining of lead, together with a few articles relating
to the mining of lead ore, which have appeared in the _Engineering and
Mining Journal_, chiefly during the last three years; in a few cases
articles from earlier issues have been inserted, in view of their
special importance in rounding out certain of the subjects treated.
For the same reason, several articles from the _Transactions_ of
the American Institute of Mining Engineers have been incorporated,
permission to republish them in this way having been courteously
granted by the Secretary of the Institute. Certain of the other
articles comprised in this book are abstracts of papers originally
presented before engineering societies, or published in other technical
periodicals, subsequently republished in the _Engineering and Mining
Journal_, as to which proper acknowledgment has been made in all cases.
The articles comprised in this book relate to a variety of subjects,
which are of importance in the practical metallurgy of lead, and
especially in connection with the desulphurization of galena, which is
now accomplished by a new class of processes known as “Lime Roasting”
processes. The successful introduction of these processes into the
metallurgy of lead has been one of the most important features in
the history of the latter during the last twenty-five years. Their
development is so recent that they are not elsewhere treated in
technical literature, outside of the pages of the periodicals and the
transactions of engineering societies. The theory and practice of these
processes are not yet by any means well understood, and a year or two
hence we shall doubtless possess much more knowledge concerning them
than we have now. Prompt information respecting such new developments
is, however, more desirable than delay with a view to saying the
last word on the subject, which never can be said by any of us, even
if we should wait to the end of the lifetime. For this reason it
has appeared useful to collect and republish in convenient form the
articles of this character which have appeared during the last few
years.
W. R. INGALLS.
AUGUST 1, 1906.
CONTENTS
PART I
NOTES ON LEAD MINING
PAGE
SOURCES OF LEAD PRODUCTION IN THE UNITED STATES (WALTER
RENTON INGALLS) 3
NOTES ON THE SOURCE OF THE SOUTHEAST MISSOURI LEAD (H. A.
WHEELER) 10
MINING IN SOUTHEASTERN MISSOURI (WALTER RENTON INGALLS) 16
LEAD MINING IN SOUTHEASTERN MISSOURI (R. D. O. JOHNSON) 18
THE LEAD ORES OF SOUTHWESTERN MISSOURI (C. V. PETRAEUS AND
W. GEO. WARING) 24
PART II
ROAST-REACTION SMELTING
SCOTCH HEARTHS AND REVERBERATORY FURNACES
LEAD SMELTING IN THE SCOTCH HEARTH (KENNETH W. M. MIDDLETON) 31
THE FEDERAL SMELTING WORKS, NEAR ALTON, ILL. (O. PUFAHL) 38
LEAD SMELTING AT TARNOWITZ (EDITORIAL) 41
LEAD SMELTING IN REVERBERATORY FURNACES AT DESLOGE, MO.
(WALTER RENTON INGALLS) 42
PART III
SINTERING AND BRIQUETTING
THE DESULPHURIZATION OF SLIMES BY HEAP ROASTING AT BROKEN
HILL (E. J. HORWOOD) 51
THE PREPARATION OF FINE MATERIAL FOR SMELTING (T. J. GREENWAY) 59
THE BRIQUETTING OF MINERALS (ROBERT SCHORR) 63
A BRICKING PLANT FOR FLUE DUST AND FINE ORES (JAS. C. BENNETT) 66
PART IV
SMELTING IN THE BLAST FURNACE
MODERN SILVER-LEAD SMELTING (ARTHUR S. DWIGHT) 73
MECHANICAL FEEDING OF SILVER-LEAD BLAST FURNACES (ARTHUR S.
DWIGHT) 81
COST OF SMELTING AND REFINING (MALVERN W. ILES) 96
SMELTING ZINC RETORT RESIDUES (E. M. JOHNSON) 104
ZINC OXIDE IN SLAGS (W. MAYNARD HUTCHINGS) 108
PART V
LIME-ROASTING OF GALENA
THE HUNTINGTON-HEBERLEIN PROCESS 113
LIME-ROASTING OF GALENA (EDITORIAL) 114
THE NEW METHODS OF DESULPHURIZING GALENA (W. BORCHERS) 116
LIME-ROASTING OF GALENA (W. MAYNARD HUTCHINGS) 126
THEORETICAL ASPECTS OF LEAD-ORE ROASTING (C. GUILLEMAIN) 133
METALLURGICAL BEHAVIOR OF LEAD SULPHIDE AND CALCIUM SULPHATE
(F. O. DOELTZ) 139
THE HUNTINGTON-HEBERLEIN PROCESS (DONALD CLARK) 144
THE HUNTINGTON-HEBERLEIN PROCESS AT FRIEDRICHSHÜTTE (A.
BIERNBAUM) 148
THE HUNTINGTON-HEBERLEIN PROCESS FROM THE HYGIENIC STANDPOINT
(A. BIERNBAUM) 160
THE HUNTINGTON-HEBERLEIN PROCESS (THOMAS HUNTINGTON AND
FERDINAND HEBERLEIN) 167
MAKING SULPHURIC ACID AT BROKEN HILL (EDITORIAL) 174
THE CARMICHAEL-BRADFORD PROCESS (DONALD CLARK) 175
THE CARMICHAEL-BRADFORD PROCESS (WALTER RENTON INGALLS) 177
THE SAVELSBERG PROCESS (WALTER RENTON INGALLS) 186
LIME-ROASTING OF GALENA (WALTER RENTON INGALLS) 193
PART VI
OTHER METHODS OF SMELTING
THE BORMETTES METHOD OF LEAD AND COPPER SMELTING (ALFREDO
LOTTI) 215
THE GERMOT PROCESS (WALTER RENTON INGALLS) 224
PART VII
DUST AND FUME RECOVERY
FLUES, CHAMBERS AND BAG-HOUSES
DUST CHAMBER DESIGN (MAX J. WELCH) 229
CONCRETE IN METALLURGICAL CONSTRUCTION (HENRY W. EDWARDS) 234
CONCRETE FLUES (EDWIN H. MESSITER) 240
CONCRETE FLUES (FRANCIS T. HAVARD) 242
BAG-HOUSES FOR SAVING FUME (WALTER RENTON INGALLS) 244
PART VIII
BLOWERS AND BLOWING ENGINES
ROTARY BLOWERS VS. BLOWING ENGINES FOR LEAD SMELTING (EDITORIAL) 251
ROTARY BLOWERS VS. BLOWING ENGINES (J. PARKE CHANNING) 254
BLOWERS AND BLOWING ENGINES FOR LEAD AND COPPER SMELTING
(HIRAM W. HIXON) 256
BLOWING ENGINES AND ROTARY BLOWERS (S. E. BRETHERTON) 258
PART IX
LEAD REFINING
THE REFINING OF LEAD BULLION (F. L. PIDDINGTON) 263
THE ELECTROLYTIC REFINING OF BASE LEAD BULLION (TITUS ULKE) 270
ELECTROLYTIC LEAD REFINING (ANSON G. BETTS) 274
PART X
SMELTING WORKS AND REFINERIES
THE NEW SMELTER AT EL PASO, TEXAS (EDITORIAL) 285
NEW PLANT OF THE AMERICAN SMELTING AND REFINING COMPANY AT
MURRAY, UTAH (WALTER RENTON INGALLS) 287
THE MURRAY SMELTER, UTAH (O. PUFAHL) 291
THE PUEBLO LEAD SMELTERS (O. PUFAHL) 294
THE PERTH AMBOY PLANT OF THE AMERICAN SMELTING AND REFINING
COMPANY (O. PUFAHL) 296
THE NATIONAL PLANT OF THE AMERICAN SMELTING AND REFINING
COMPANY (O. PUFAHL) 299
THE EAST HELENA PLANT OF THE AMERICAN SMELTING AND REFINING
COMPANY (O. PUFAHL) 302
THE GLOBE PLANT OF THE AMERICAN SMELTING AND REFINING COMPANY
(O. PUFAHL) 304
LEAD SMELTING IN SPAIN (HJALMAR ERIKSSON) 306
LEAD SMELTING AT MONTEPONI, SARDINIA (ERMINIO FERRARIS) 311
PART I
NOTES ON LEAD MINING
SOURCES OF LEAD PRODUCTION IN THE UNITED STATES
BY WALTER RENTON INGALLS
(November 28, 1903)
Statistics of lead production are of value in two directions: (1) in
showing the relative proportion of the kinds of lead produced; and (2)
in showing the sources from which produced. Lead is marketed in three
principal forms: (_a_) desilverized; (_b_) soft; (_c_) antimonial, or
hard. The terms to distinguish between classes “a” and “b” are inexact,
because, of course, desilverized lead is soft lead. Desilverized lead
itself is classified as “corroding,” which is the highest grade, and
ordinary “desilverized.” Soft lead, referring to the Missouri product,
may be either “ordinary” or “chemical hard.” The latter is such lead
as contains a small percentage of copper and antimony as impurities,
which, without making it really hard, increase its resistance against
the action of acids, and therefore render it especially suitable
for the production of sheet to be used in sulphuric-acid chamber
construction and like purposes. The production of chemical hard lead
is a fortuitous matter, depending on the presence of the valuable
impurities in the virgin ores. If present, these impurities go into
the lead, and cannot be completely removed by the simple process of
refining which is practised. Nobody knows just what proportions of
copper and antimony are required to impart the desired property, and
consequently no specifications are made. Some chemical engineers call
for a particular brand, but this is really only a whim, since the same
brand will not be uniformly the same; practically one brand is as good
as another. Corroding lead is the very pure metal, which is suitable
for white lead manufacture. It may be made either from desilverized or
from the ordinary Missouri product; or the latter, if especially pure,
may be classed as corroding without further refining. Antimonial lead
is really an alloy of lead with about 15 to 30 per cent. antimony,
which is produced as a by-product by the desilverizers of base
bullion. The antimony content is variable, it being possible for the
smelter to run the percentage up to 60. Formerly it was the general
custom to make antimonial lead with a content of 10 to 12 per cent. Sb;
later, with 18 to 20 per cent.; while now 25 to 30 per cent. Sb is best
suited to the market.
The relative values of the various grades of lead fluctuate
considerably, according to the market place, and the demand and supply.
The schedules of the American Smelting and Refining Company make a
regular differential of 10c. per 100 lb. between corroding lead and
desilverized lead in all markets. In the St. Louis market, desilverized
lead used to command a premium of 5c. to 10c. per 100 lb. over ordinary
Missouri; but now they sell on approximately equal terms. Chemical hard
lead sells sometimes at a higher price, sometimes at a lower price,
than ordinary Missouri lead, according to the demand and supply. There
is no regular differential. This is also the case with antimonial
lead.[1]
The total production of lead from ores mined in the United States in
1901 was 279,922 short tons, of which 211,368 tons were desilverized,
57,898 soft (meaning lead from Missouri and adjacent States) and
10,656 antimonial. These are the statistics of “The Mineral Industry.”
The United States Geological Survey reported substantially the same
quantities. In 1902 the production was 199,615 tons of desilverized,
70,424 tons of soft, and 10,485 tons of antimonial, a total of 280,524
tons. There is an annual production of 4000 to 5000 tons of white
lead direct from ore at Joplin, Mo., which increases the total lead
production of the United States by, say, 3500 tons per annum. The
production of lead reported as “soft” does not represent the full
output of Missouri and adjacent States, because a good deal of their
ore, itself non-argentiferous, except to the extent of about 1 oz. per
ton in certain districts, is smelted with silver-bearing ores, going
thus into an argentiferous lead; while in one case, at least, the
almost non-argentiferous lead, obtained by smelting the ore unmixed, is
desilverized for the sake of the extra refining.
Lead-bearing ores are of widespread occurrence in the United States.
Throughout the Rocky Mountains there are numerous districts in which
the ore carries more or less lead in connection with gold and silver.
For this reason, the lead mining industry is not commonly thought of as
having such a concentrated character as copper mining and zinc mining.
It is the fact, however, that upward of 70 per cent. of the lead
produced in the United States is derived from five districts, and in
the three leading districts from a comparatively small number of mines.
The statistics of these for 1901 to 1904 are as follows:[2]
┌──────────┬───────────────────────────────┬───────────────────────┬────
│ │ PRODUCTION, TONS │ PER CENT. │
│DISTRICT │ 1901 │ 1902 │ 1903 │ 1904 │ 1901│ 1902│ 1903│ 1904│REF.
├──────────┼───────┼───────┼───────┼───────┼─────┼─────┼─────┼─────┼────
│Cœur │ │ │ │ │ │ │ │ │
│d’Alene │ 68,953│ 74,739│ 89,880│ 98,240│ 24.3│ 26.3│ 32.5│ 32.5│_a_
│Southeast │ │ │ │ │ │ │ │ │
│Mo. │ 46,657│ 56,550│ 59,660│ 59,104│ 16.4│ 19.9│ 21.2│ 19.6│_b_
│Leadville,│ │ │ │ │ │ │ │ │
│Colo. │ 28,180│ 19,725│ 18,177│ 23,590│ 10.0│ 6.9│ 6.6│ 7.8│_c_
│Park City,│ │ │ │ │ │ │ │ │
│Utah │ 28,310│ 36,300│ 36,534│ 30,192│ 10.0│ 12.8│ 13.2│ 10.0│_d_
│Joplin, │ │ │ │ │ │ │ │ │
│Mo.-Kan. │ 24,500│ 22,130│ 20,000│ 23,600│ 8.6│ 7.8│ 7.2│ 7.8│_e_
│ ├───────┼───────┼───────┼───────┼─────┼─────┼─────┼─────┤
│ Total │196,600│209,444│224,251│234,726│ 69.3│ 73.7│ 81.0│ 77.7│
_a._ The production in 1901 and 1902 is computed from direct returns
from the mines, with an allowance of 6 per cent. for loss of lead in
smelting. The production in 1903 and 1904 is estimated at 95 per cent.
of the total lead product of Idaho.
_b._ This figure includes only the output of the mines at Bonne Terre,
Flat River, Doe Run, Mine la Motte and Fredericktown. It is computed
from the report of the State Lead and Zinc Mine Inspector as to ore
produced, the ore (concentrates) of the mines at Bonne Terre, Flat
River and Doe Run being reckoned as yielding 60 per cent. lead.
_c._ Report of State Commissioner of Mines.
_d._ Report of Director of the Mint on “Production of Gold and Silver
in the United States,” with allowance of 6 per cent. for loss of lead
in smelting.
_e._ From statistics reported by “The Mineral Industry,” reckoning the
ore (concentrates) as yielding 70 per cent. lead.
Outside of these five districts, the most of the lead produced in the
United States is derived from other camps in Idaho, Colorado, Missouri
and Utah, the combined output of all other States being insignificant.
It is interesting to examine the conditions under which lead is
produced in the five principal districts.
_Leadville, Colo._—The mines of Leadville, which once were the largest
lead producers of the United States, became comparatively unimportant
after the exhaustion of the deposits of carbonate ore, but have
attained a new importance since the successful introduction of means
for separating the mixed sulphide ore, which occurs there in very large
bodies. The lead production of Leadville in 1897 was 11,850 tons;
17,973 tons in 1898; 24,299 tons in 1899; 31,300 tons in 1900; 28,180
tons in 1901, and 19,725 tons in 1902. The Leadville mixed sulphide ore
assays about 8 per cent. Pb, 25 per cent. Zn and 10 oz. silver per ton.
It is separated into a zinc product assaying about 38 per cent. Zn and
6 per cent. Pb, and a galena product assaying about 45 per cent. Pb, 10
or 12 per cent. Zn, and 10 oz. silver per ton.
_Cœur d’Alene._—The mines of this district are opened on fissure veins
of great extent. The ore is of low grade and requires concentration. As
mined, it contains about 10 per cent. lead and a variable proportion
of silver. It is marketed as mineral, averaging about 50 per cent. Pb
and 30 oz. silver per ton. The production of lead ore in this district
is carried on under the disadvantages of remoteness from the principal
markets for pig lead, high-priced labor, and comparatively expensive
supplies. It enjoys the advantages of large orebodies of comparatively
high grade in lead, and an important silver content, and in many cases
cheap water power, and the ability to work the mines through adit
levels. The cost of mining and milling a ton of crude ore is $2.50 to
$3.50. The mills are situated, generally, at some distance from the
mines, the ore being transported by railway at a cost of 8 to 20c.
per ton. The dressing is done in large mills at a cost of 40 to 50c.
per ton. About 75 per cent. of the lead of the ore is recovered. The
concentrates are sold at 90 per cent. of their lead contents and 95 per
cent. of their silver contents, less a smelting charge of $8 per ton,
and a freight rate of $8 per ton on ore of less than $50 value per ton,
$10 on ore worth $50 to $65, and $12 on ore worth more than $65; the
ore values being computed f. o. b. mines. The settling price of lead is
the arbitrary one made by the American Smelting and Refining Company.
With lead (in ore) at 3.5c. and silver at 50c., the value, f. o. b.
mines, of a ton of ore containing 50 per cent. Pb and 30 oz. silver is
approximately as follows:
1000 × 0.90 = 900 lb. lead, at 3.5c. $31.50
30 × 0.95 = 28.5 oz. silver, at 50c. 14.25
——————
Gross value, f. o. b. mines $45.75
Less freight, $10, and smelting charge, $8 18.00
——————
Net value, f. o. b. mines $27.75
Assuming an average of 6 tons of crude ore to 1 ton of concentrate, the
value per ton of crude ore would be about $4.62½, and the net profit
per ton about $1.62½, which figures are increased 23.75c. for each 5c.
rise in the value of silver above 50c. per ounce.
The production of the Cœur d’Alene since 1895, as reported by the
mines, has been as follows:
─—─—─—-———─—─┬—─—-——————─—─┬—─—-—————————┬——————─—─
YEAR │ LEAD, TONS │ SILVER, OZ. │ RATIO[3]
─—─—─—-———─—─┼—─—-——————─—─┼—─—-—————————┼——————─—─
1896 │ 37,250 │ 2,500,000 │ 67.1
1897 │ 57,777 │ 3,579,424 │ 61.9
1898 │ 56,339 │ 3,399,524 │ 60.3
1899 │ 50,006 │ 2,736,872 │ 54.7
1900 │ 81,535 │ 4,755,877 │ 58.3
1901 │ 68,953 │ 3,349,533 │ 48.5
1902 │ 74,739 │ 4,489,549 │ 60.0
1903 │ [4]100,355 │ 5,751,613 │ 57.3
1904 │ [4]108,954 │ 6,247,795 │ 57.4
─—─—─—-———─—─┴—─—-——————─—─┴—─—-—————————┴——————─—─
The number of producers in the Cœur d’Alene district is comparatively
small, and many of them have recently consolidated, under the name of
the Federal Mining and Smelting Company. Outside of that concern are
the Bunker Hill & Sullivan, the Morning and the Hercules mines, control
of which has lately been secured by the American Smelting and Refining
Company.
_Southeastern Missouri._—The most of the lead produced in this region
comes from what is called the disseminated district, comprising
the mines of Bonne Terre, Flat River, Doe Run, Mine la Motte and
Fredericktown, of which those of Bonne Terre and Flat River are the
most important. The ore of this region is a magnesian limestone
impregnated with galena. The deposits lie nearly flat and are very
large. They yield about 5 per cent. of mineral, which assays about 65
per cent. lead. The low grade of the ore is the only disadvantage which
this district has, but this is so much more than offset by the numerous
advantages, that mining is conducted very profitably, and it is an open
question whether lead can be produced more cheaply here or in the Cœur
d’Alene. The mines of southeastern Missouri are only 60 to 100 miles
distant from St. Louis, and are in close proximity to the coalfields
of southern Illinois, which afford cheap fuel. The ore lies at depths
of only 100 to 500 ft. below the surface. The ground stands admirably,
without any timbering. Labor and supplies are comparatively cheap.
Mining and milling can be done for $1.05 to $1.25 per ton of crude ore,
when conducted on the large scale that is common in this district.
Most of the mining companies are equipped to smelt their own ore, the
smelters being either at the mines or near St. Louis. The freight rate
on concentrates to St. Louis is $1.40 per ton; on pig lead it is $2.10
per ton. The total cost of producing pig lead, delivered at St. Louis,
is about 2.25c. per pound, not allowing for interest on the investment,
amortization, etc.
The production of the mines in the disseminated district in 1901 was
equivalent to 46,657 tons of pig lead; in 1902 it was 56,550 tons. The
milling capacity of the district is about 6000 tons per day, which
corresponds to a capacity for the production of about 57,000 tons of
pig lead per annum. The St. Joseph Lead Company is building a new 1000
ton mill, and the St. Louis Smelting and Refining Company (National
Lead Company) is further increasing its output, which improvements will
increase the daily milling capacity by about 1400 tons, and will enable
the district to put out upward of 66,000 tons of pig lead. In this
district, as in the Cœur d’Alene, the industry is closely concentrated,
there being only nine producers, all told.
_Park City, Utah._—Nearly all the lead produced by this camp comes
from the Silver King, Daly West, Ontario, Quincy, Anchor and Daly
mines, which have large veins of low-grade ore carrying argentiferous
galena and blende, a galena product being obtained by dressing, and
zinkiferous tailings, which are accumulated for further treatment as
zinc ore, when market conditions justify.[5]
_Joplin District._—The lead production of southwestern Missouri and
southeastern Kansas, in what is known as the Joplin district, is
derived entirely as a by-product in dressing the zinc ore of that
district. It is obtained as a product assaying about 77 per cent. Pb,
and is the highest grade of lead ore produced, in large quantity,
anywhere in the United States. It is smelted partly for the production
of pig lead, and partly for the direct manufacture of white lead. The
lead ore production of the district was 31,294 tons in 1895, 26,927
tons in 1896, 29,578 tons in 1897, 26,457 tons in 1898, 24,100 tons
in 1899, 28,500 tons in 1900, 35,000 tons in 1901, and 31,615 tons in
1902. The production of lead ore in this district varies more or less,
according to the production of zinc ore, and is not likely to increase
materially over the figure attained in 1901.
NOTES ON THE SOURCE OF THE SOUTHEAST MISSOURI LEAD
BY H. A. WHEELER
(March 31, 1904)
The source of the lead that is being mined in large quantities in
southeastern Missouri has been a mooted question. Nor is the origin
of the lead a purely theoretical question, as it has an important
bearing on the possible extension of the orebodies into the underlying
sandstone.
The disseminated lead ores of Missouri occur in a shaly, magnesian
limestone of Cambrian age in St. François, Madison and Washington
counties, from 60 to 130 miles south of St. Louis. The limestone
is known as the Bonne Terre, or lower half of “the third magnesian
limestone” of the Missouri Geological Survey, and rests on a sandstone,
known as “the third sandstone,” that is the base of the sedimentary
formations in the area. Under this sandstone occur the crystalline
porphyries and granites of Algonkian and Archean age, which outcrop as
knobs and islands of limited extent amid the unaltered Cambrian and
Lower Silurian sediments.
The lead occurs as irregular granules of galena scattered through the
limestone in essentially horizontal bodies that vary from 5 to 100
ft. in thickness, from 25 to 500 ft. in width, and have exceeded 9000
ft. in length. There is no vein structure, no crushing or brecciation
of the inclosing rock, yet these orebodies have well defined axes or
courses, and remarkable reliability and persistency. It is true that
the limestone is usually darker, more porous, and more apt to have thin
seams of very dark (organic) shales where it is ore-bearing than in the
surrounding barren ground. The orebodies, however, fade out gradually,
with no sharp line between the pay-rock and the non-paying, and the
lead is rarely, if ever, entirely absent in any extent of the limestone
of the region. While the main course of the orebodies seems to be
intimately connected with the axes of the gentle anticlinal folds,
numerous cross-runs of ore that are associated with slight faults are
almost as important as the main shoots, and have been followed for
5000 ft. in length. These cross-runs are sometimes richer than the
main runs, at least near the intersections, but they are narrower, and
partake more of the type of vertical shoots, as distinguished from the
horizontal sheet-form.
Most of the orebodies occur at, or close to, the base of the limestone,
and frequently in the transition rock between the underlying sandstone
and the limestone, though some notable and important bodies have
been found from 100 to 200 ft. above the sandstone. This makes the
working depth from the surface vary from 150 to 250 ft., for the upper
orebodies, to 300 to 500 ft. deep to the main or basal orebodies,
according as erosion has removed the ore-bearing limestone. The
thickness of the latter ranges from 400 to 500 ft.
Associated with the galena are less amounts of pyrite, which especially
fringes the orebodies, and very small quantities of chalcopyrite, zinc
blende, and siegenite (the double sulphide of nickel and cobalt).
Calcite also occurs, especially where recent leaching has opened
vugs, caves, or channels in the limestone, when secondary enrichment
frequently incrusts these openings with crystals of calcite and galena.
No barite ever occurs with the disseminated ore, though it is the
principal gangue mineral in the upper or Potosi member of the third
magnesian limestone, and is never absent in the small ore occurrences
in the still higher second magnesian limestone.
While the average tenor of the ore is low, the yield being from 3 to
4 per cent. in pig lead, they are so persistent and easy to mine that
the district today is producing about 70,000 tons of pig lead annually,
and at a very satisfactory profit. As the output was about 2500 tons
lead in 1873, approximately 8500 tons in 1883, and about 20,000 tons in
1893, it shows that this district is young, for the principal growth
has been within the last five years.
Of the numerous but much smaller occurrences of lead elsewhere in
Missouri and the Mississippi valley, none resembles this district
in character, a fact which is unique. For while the Mechernich lead
deposits, in Germany, are disseminated, and of even lower grade than in
Missouri, they occur in a sandstone, and (like all the lead deposits
outside of the Mississippi valley) they are argentiferous, at least to
an extent sufficient to make the extraction of the silver profitable;
and on the non-argentiferous character of the disseminated deposits
hangs my story.
Of the numerous hypotheses advanced to account for the origin of these
deposits, there are only two that seem worthy of consideration: (a)
the _lateral secretion theory_, and (b) _deposition from solutions of
deep-seated origin_. Other theories evolved in the pioneer period of
economic geology are interesting, chiefly by reason of the difficulties
under which the early strugglers after geological knowledge blazed the
pathway for modern research and observation.
The lateral secretion theory, as now modernized into the secondary
enrichment hypothesis, has much merit when applied to the southeastern
and central Missouri lead deposits. For the limestones throughout
Missouri—and they are the outcropping formation over more than half of
the State—are rarely, if ever, devoid of at least slight amounts of
lead and zinc, although they range in age from the Carboniferous down
to the Cambrian.
The sub-Carboniferous formation is almost entirely made up of
limestones, which aggregate 1200 to 1500 ft. in thickness. They
frequently contain enough lead (and less often zinc) to arouse the
hopes of the farmer, and more or less prospecting has been carried on
from Hannibal to St. Louis, or 125 miles along the Mississippi front,
and west to the central part of the State, but with most discouraging
results.
In the rock quarries of St. Louis, immediately under the lower coal
measures, fine specimens of millerite of world-wide reputation occur
as filiform linings of vugs in this sub-Carboniferous limestone. These
vugs occur in a solid, unaltered rock which gives no clue to the
existence of the vug or cavity until it is accidentally broken. The
vugs are lined with crystals of pink dolomite, calcite and millerite,
with occasionally barite, selenite, galena and blende. They occur
in a well-defined horizon about 5 ft. thick, and the vugs in the
limestone above and below this millerite bed contain only calcite,
or less frequently dolomite. Yet this sub-Carboniferous formation in
southwestern Missouri, about Joplin, carries the innumerable pockets
and sheets of lead and zinc that have made that district the most
important zinc producer in the world. While faulting and limited
folding occur in eastern and central Missouri to fully as great an
extent as in St. François county or the Joplin district, thus far no
mineral concentration into workable orebodies has been found in this
formation, except in the Joplin area.
The next important series of limestones that make up most of the
central portion of Missouri are of Silurian age, and in them lead and
zinc are liberally scattered over large areas. In the residual surface
clays left by dissolution of the limestone, the farmers frequently make
low wages by gophering after the liberated lead, and the aggregate
of these numerous though insignificant gopher-holes makes quite a
respectable total. But they are only worked when there is nothing else
to do on the farm, as with rare exceptions they do not yield living
wages, and the financial results of mining the rock are even less
satisfactory. Yet a few small orebodies have been found that were
undoubtedly formed by local leaching and re-precipitation of this
diffused lead and zinc. Such orebodies occur in openings or caves,
with well crystallized forms of galena and blende, and invariably
associated with crystallized “tiff” or barite. I am not aware of any
of these pockets or secondary enrichments having produced as much as
2000 tons of lead or zinc, and very few have produced as much as 500
tons, although one of these pockets was recently exploited with heroic
quantities of printer’s ink as the largest lead mine in the world. Yet
there are large areas in which it is almost impossible to put down a
drill-hole without finding “shines” or trifling amounts of lead or
zinc. That these central Missouri lead deposits are due to lateral
secretion there seems little doubt, and it is possible that larger
pockets may yet be found where more favorable conditions occur.
When the lateral secretion theory is applied to the disseminated
deposits of southeastern Missouri, we are confronted by enormous bodies
of ore, absence of barite, non-crystallized condition of the galena
except in local, small, evidently secondary deposits, and well-defined
courses for the main and cross-runs of ore. The Bonne Terre orebody,
which has been worked longest and most energetically, has attained a
length of nearly 9000 ft., with a production of about 350,000 tons
or $30,000,000 of lead, and is far from being exhausted. Orebodies
recently opened are quite as promising. The country rock is not as
broken nor as open as in central Missouri, and is therefore much less
favorable for the lateral circulation of mineral waters, yet the
orebodies vastly exceed those of the central region.
Further, the Bonne Terre formation is heavily intercalated with thick
sheets of shale that would hinder overlying waters from reaching the
base of the ore-horizon, where most of the ore occurs, so that the
leachable area would be confined to a very limited vertical range,
or to but little greater thickness than the 100 ft. or so in which
most of the orebodies occur. While I have always felt that such large
bodies, showing relatively rapid precipitation of the lead, could not
be satisfactorily explained except as having a deep-seated origin,
the fact that the disseminated ore is practically non-argentiferous,
or at least carries only one to three ounces per ton, has been a
formidable obstacle. For the lead in the small fissure-veins that
occasionally occur in the adjacent granite has always been reported
as argentiferous. Thus the Einstein silver mine, near Fredericktown,
worked a fissure-vein from 1 to 6 ft. wide in the granite. It had a
typical complex vein-filling and structure, and carried galena that
assayed from 40 to 200 oz. per ton. While the quantity of ore obtained
did not justify the expensive plant erected to operate it, the galena
was rich in silver, whereas in the disseminated ores at the Mine la
Motte mine, ten miles distant, only the customary 1.5 oz. per ton
occurs. Occasionally fine-grained specimens of galena that I have found
in the disseminated belt would unquestionably be rated as argentiferous
by a Western miner, but the assay showed that the structure in this
case was due to other causes, as only about two ounces were found.
An apparent exception was reported at the Peach Orchard diggings,
in Washington county, in the higher or Potosi member of the third
magnesian limestone, where Arthur Thacher found sulphide and carbonate
ore carrying 8 to 10 oz. of silver per ton; and a short-lived hamlet,
known as Silver City, sprang up to work them. I found, however, that
these deposits are associated with little vertical fissure-veins or
seams that unquestionably come up from the underlying porphyry.
Recently I examined the Jackson Revel mine, which has been considered
a silver mine for the last fifty years. It lies about seven miles
south of Fredericktown, and is a fissure-vein in Algonkian felsite,
where it protrudes, as a low hill, through the disseminated limestone
formation. A shaft has just been sunk about 150 ft. at less than
1000 ft. from the feather edge of the limestone. The vein is narrow,
only one to twelve inches wide, with slicken-sided walls, runs about
N. 20 deg. E., and dips 80 to 86 deg. eastward. White quartz forms
the principal part of the filling; the vein contains more or less
galena and zinc blende. Assays of the clean galena made by Prof. W. B.
Potter show only 2.5 oz. silver per ton, or no more than is frequently
found in the disseminated lead ores. As the lead in this fissure vein
may be regarded as of undoubted deep origin, and it is practically
non-argentiferous, this would seem to remove the last objection to
the theory of the deep-seated source of the lead in the disseminated
deposits of southeast Missouri.
MINING IN SOUTHEASTERN MISSOURI
BY WALTER RENTON INGALLS
(February 18, 1904)
The St. Joseph Lead Company, in the operation of its mines at Bonne
Terre, does not permit the cages employed for hoisting purposes to be
used for access to the mine. Men going to and from their work must
climb the ladders. This rule does not obtain in the other mines of the
district. The St. Joseph Lead Company employs electric haulage for
the transport of ore underground at Bonne Terre. In the other mines
of the district, mules are generally used. The flow of water in the
mines of the district is extremely variable; some have very little;
others have a good deal. The Central mine is one of the wettest in the
entire district, making about 2000 gal. of water per minute. Coal in
southeastern Missouri costs $2 to $2.25 per ton delivered at the mines,
and the cost of raising 2000 gal. of water per minute from a depth
of something like 350 ft. is a very considerable item in the cost of
mining and milling, which, in the aggregate, is expected to come to not
much over $1.25 per ton.
The ore shoots in the district are unusually large. Their precise trend
has not been identified. Some consider the predominance of trend to be
northeast; others, northwest. They go both ways, and appear to make
the greatest depositions of ore at their intersections. However, the
network of shoots, if that be the actual occurrence, is laid out on a
very grand scale. Vertically there is also a difference. Some shafts
penetrate only one stratum of ore; others, two or three. The orebody
may be only a few feet in thickness; it may be 100 ft. or more. The
occurrence of several overlying orebodies obviously indicates the
mineralization of different strata of limestone, while in the very
thick orebodies the whole zone has apparently been mineralized.
The grade of the ore is extremely variable. It may be only 1 or 2 per
cent. mineral, or it may be 15 per cent. or more. However, the average
yield for the district, in large mines which mill 500 to 1200 tons of
ore per day, is probably about 5 per cent. of mineral, assaying 65 per
cent. Pb, which would correspond to a yield of 3.25 per cent. metallic
lead in the form of concentrate. The actual recovery in the dressing
works is probably about 75 per cent., which would indicate a tenure of
about 4.33 per cent. lead in the crude ore.
LEAD MINING IN SOUTHEASTERN MISSOURI
BY R. D. O. JOHNSON
(September 16, 1905)
The lead deposits of southeastern Missouri carry galena disseminated
in certain strata of magnesian limestone. Their greater dimensions
are generally horizontal, but with outlines extremely irregular. The
large orebodies consist usually of a series of smaller bodies disposed
parallel to one another. These smaller members may coalesce, but are
generally separated from one another by a varying thickness of lean ore
or barren rock. The vertical and lateral dimensions of an orebody may
be determined with a fair degree of accuracy by diamond drilling, and a
map may be constructed from the information so obtained. Such a map (on
which are plotted the surface contours) makes it possible to determine
closely the proper location of the shaft, or shafts, considering also
the surface and underground drainage and tramming.
The first shafts in the district were sunk at Bonne Terre, where the
deposits lie comparatively near the surface. The early practice at this
point was to sink a number of small one-compartment shafts. As the
deposits were followed deeper, this gave way to the practice of putting
down two-compartment shafts equipped much more completely than were the
shallower shafts.
At Flat River (where the deposits lie at much greater depths, some
being over 500 ft.) the shafts are 7 × 14 ft., 6½ × 18 ft., and 7 × 20
ft. These larger dimensions give room not only for two cage-ways and a
ladder-way, but also for a roomy pipe-compartment. The large quantities
of water to be pumped in this part of the district make the care of
the pipes in the shafts a matter of first importance. At Bonne Terre
only such a quantity of water was encountered as could be handled by
bailing or be taken out with the rock; there the only pipe necessary
was a small air-pipe down one corner of the shaft. When the quantity
of water encountered is so great that the continued working of the mine
depends upon its uninterrupted removal, the care of the pipes becomes a
matter of great importance. A shaft which yields from 4000 to 5000 gal.
of water per minute is equipped with two 12 in. column pipes and two 4
in. steam pipes covered and sheathed. Moreover, the pipe compartment
will probably contain an 8 in. air-pipe, besides speaking-tubes, pipes
for carrying electric wires, and pipes for conducting water from upper
levels to the sump. To care for these properly there are required a
separate compartment and plenty of room.
Shafts are sunk by using temporary head frames and iron buckets of from
8 to 14 cu. ft. capacity. Where the influx of water was small, 104 ft.
have been sunk in 30 days, with three 8 hour shifts, two drills, and
two men to each drill; 2¾ in. drills are used almost exclusively; 3¼
in. drills have been used in sinking, but without apparent increase in
speed.
The influence of the quantity of water encountered upon the speed of
sinking (and the consequent cost per foot) is so great that figures are
of little value. Conditions are not at all uniform.
At some point (usually before 200 ft. is reached) a horizontal opening
will be encountered. This opening invariably yields water, the amount
following closely the surface precipitation. It is the practice to
establish at this point a pumping station. The shaft is “ringed” and
the water is directed into a sump on the side, from which it is pumped
out. This sump receives also the discharge of the sinking pumps.
The shafts sunk in solid limestone require no timbering other than that
necessary to support the guides, pipes, and ladder platforms. These
timbers are 8 × 8 in. and 6 x 8 in., spaced 7 or 8 ft. apart.
Shafts are sunk to a depth of 10 ft. below the point determined upon
as the lower cage landing. From the end at the bottom a narrow drift
is driven horizontally to a distance of 15 ft.; at that point it is
widened out to 10 ft. and driven 20 ft. further. The whole area (10 ×
20 ft.) is then raised to a point 28 or 30 ft. above the bottom of the
drift from the shaft. The lower part of this chamber constitutes the
sump. Starting from this chamber (on one side and at a point 10 ft.
above the cage landing, or 20 ft. above the bottom of the sump), the
“pump-house” is cut out. This pump-house is cut 40 ft. long and is as
wide as the sump is long, namely, 20 ft. A narrow drift is driven to
connect the top of the pump-house with the shaft. Through this drift
the various pipes enter the pump-house from the shaft.
The pumps are thus placed at an elevation of 10 ft. above the bottom
of the mine. Flooding of mines, due to failure of pumps or to striking
underground bodies of water, taught the necessity of placing the pumps
at such an elevation that they would be the last to be covered, thus
giving time for getting or keeping them in operation. The pumps are
placed on the solid rock, the air pumps and condensers at a lower level
on timbers over the sump.
With this arrangement, the bottom of the shaft serves as an antechamber
for the sump, in which is collected the washing from the mine and the
dripping from the shaft. The sump proper rarely needs cleaning.
The pumps are generally of high-grade, compound-and triple-expansion,
pot-valved, outside-packed plunger pattern. Plants with electrical
power distribution have recently installed direct-connected compound
centrifugal pumps with entire success.
Pumps of the Cornish pattern have never been used much in this region.
One such pump has been installed, but the example has not been followed
even by the company putting it in.
The irregular disposition of the ore renders any systematic plan of
drifting or mining (as in coal or vein mining) impossible. On each
side of the shaft and in a direction at right angles to its greater
horizontal dimension, drifts 12 to 14 ft. in width are driven to a
distance of 60 or 70 ft. In these broad drifts are located the tracks
and also the “crossovers” for running the cars on and off the cage.
When a deposit is first opened up, it is usually worked on two, and
sometimes three, levels. These eventually cut into one another, when
the ore is hoisted from the lower level alone.
The determination of the depth of the lower level is a matter of
compromise. Much good ore may be known to exist below; when it comes
to mining, it will have to be taken out at greater expense; but the
level is aimed to cut through the lower portions of the main body. It
is generally safe to predict that the ore lying below the upper levels
will eventually be mined from a lower level without the expense of
local underground hoisting and pumping.
The ore has simply to be followed; no one can say in advance how it
is going to turn out. The irregularity of the deposits renders any
general plan of mining of little or no value. Some managers endeavor to
outline the deposits by working on the outskirts, leaving the interior
as “ore reserves.” Such reserves have been found to be no reserves at
all, though the quality of the rock may be fairly well determined by
underground diamond drilling. Many of the deposits are too narrow to
permit the employment of any system of outlining and at the same time
keeping up the ore supply.
The individual bodies constituting the general orebody are rarely,
if ever, completely separated by barren rock; some “stringers” or
“leaders” of ore connect them. The careful superintendent keeps a
record on the monthly mine map of all such occurrences, or otherwise,
or of blank walls of barren rock that mark the edge of the deposit.
This precaution finds abundant reward when the drills commence to “cut
poor,” and when a search for ore is necessary.
The method of mining is to rise to the top of the ore and to carry
forward a 6 ft. breast. If the ore is thick enough, this is followed by
the underhand stope. Drill holes in the breast are usually 7 or 8 ft.
in depth; stope holes, 10 to 14 feet.
Both the roof and the floor are drilled with 8 or 10 ft. holes placed
8 or 10 ft. apart. These serve to prospect the rock in the immediate
neighborhood; in the roof they serve the further very important purpose
of draining out water that might otherwise accumulate between the
strata and that might force them to fall. The condition or safety
of the roof is determined by striking with a hammer. If the sound
is hollow or “drummy,” the roof is unsafe. If water is allowed to
accumulate between the loose strata, obviously it is not possible to
determine the condition of the roof.
It is the duty of two men on each shift to keep the mine in a safe
condition by taking down all loose and dangerous masses of rock. These
men are known as “miners.” It sometimes happens that a considerable
area of the roof gets into such a dangerous condition that it is either
too risky or too expensive to put in order, in which case the space
underneath is fenced off. As a general thing, the mines are safe and
are kept so. There are but few accidents of a serious nature due to
falling rock.
The roof is supported entirely by pillars; no timbering whatever is
used. The pillars are parts of the orebody or rock that is left. They
are of all varieties of size and shape. They are usually circular in
cross-section, 10 to 15 ft. in diameter and spaced 20 to 35 ft. apart,
depending upon the character of the roof. Pillars generally flare at
the top to give as much support to the roof as possible. The hight of
the pillars corresponds, of course, to the thickness of the orebody.
All drilling is done by 2¾ in. percussion drills. In the early days,
when diamonds were worth $6 per carat, underground diamond drills were
used. Diamond drills are used now occasionally for putting in long
horizontal holes for shooting down “drummy” roof. Air pressure varies
from 60 to 80 lb. Pressures of 100 lb. and more have been used, but the
repairs on the drills became so great that the advantages of the higher
pressure were neutralized.
Each drill is operated by two men, designated as “drillers,” or “front
hand” and “back hand.” The average amount of drilling per shift of 10
hours is in the neighborhood of 40 ft., though at one mine an average
of 55 ft. was maintained.
In some of the mines the “drillers” and “back hands” do the loading and
firing; in others that is done by “firers,” who do the blasting between
shifts. When the drillers do the firing, there is employed a “powder
monkey,” who makes up the “niphters,” or sticks of powder, in which are
inserted and fastened the caps and fuse; 35 per cent. powder is used
for general mining.
Battery firing is employed only in shaft sinking. In the mining work
this is found to be much more expensive; the heavy concussions loosen
the stratum of the roof and make it dangerous.
Large quantities of oil are used for lubrication and illumination.
“Zero” black oil and oils of that grade are used on the drills. Miners’
oil is generally used for illumination, though some of the mines use a
low grade of felsite wax.
Two oil cans (each holding about 1½ pints) are given to each pair of
drillers, one can for black oil and one for miners’ oil. These cans,
properly filled, are given out to the men, as they go on shift, at the
“oil-house,” located near the shaft underground. This “oil-house” is in
charge of the “oil boy,” whose duty it is to keep the cans clean, to
fill them and to give them out at the beginning of the shift. The cans
are returned to the oil-house at the end of the shift.
Kerosene is used in the hat-lamps in wet places.
The “oil-houses” are provided with three tanks. In some instances these
tanks are charged through pipes coming down the shaft from the surface
oil-house. These tanks are provided with oil-pumps and graduated
gage-glasses.
Shovelers or loaders operate in gangs of 8 to 12, and are supervised by
a “straw boss,” who is provided with a gallon can for illuminating oil.
The cars are 20 cu. ft. (1 ton) capacity. Under ordinary conditions one
shoveler will load 20 of these cars in a shift of 10 hours. They use
“half-spring,” long-handled, round-pointed shovels.
Cars are of the solid-box pattern, and are dumped in cradles. Loose
and “Anaconda” manganese-steel wheels are the most common. Gage of
track, 24 to 30 in., 16 lb. rails on main lines and 12 lb. on the side
and temporary tracks. Cars are drawn by mules. One mine has installed
compressed-air locomotives and is operating them with success.
Shafts are generally equipped with geared hoists, both steam and
electrically driven. Later hoists are all of the first-motion pattern.
Generally the cars are hoisted to the top and dumped with cradles. One
shaft, however, is provided with a 5-ton skip, charged at the bottom
from a bin, into which the underground cars are dumped. Upon arriving
at the top the skip dumps automatically. This design exhibits a number
of advantages over the older method and will probably find favor with
other mine operators.
THE LEAD ORES OF SOUTHWESTERN MISSOURI
BY C. V. PETRAEUS AND W. GEO. WARING
(October 21, 1905)
The lead ore of southwestern Missouri, and the adjoining area in the
vicinity of Galena, Kan., is obtained as a by-product of zinc mining,
the galena being separated from the blende in the jigging process.
Formerly the galena (together with “dry-bone,” including cerussite and
anglesite) was the principal ore mined from surface deposits in clay,
the blende being the subsidiary product. In the deeper workings blende
was found largely to predominate; this is shown by the shipments of the
district in 1904, which amounted to 267,297 tons of zinc concentrate
and 34,533 tons of lead concentrate.
The lead occurs in segregated cubes, from less than one millimeter up
to one foot in diameter. The cleavage is perfect, so that each piece
of ore when struck with a hammer breaks up into smaller perfect cubes.
In this respect the ore differs from the galena encountered in the
Rocky Mountain regions, where torsional or shearing strains seem in
most instances to have destroyed the perfect cleavage of the minerals
subsequent to their original deposition. Cases of schistose and twisted
structure occur in lead deposits of the Joplin district but rarely, and
they are always quite local.
The separation of the galena from the blende and marcasite (“mundic”)
in the ordinary process of jigging is very complete; the percentage
of zinc and iron in the lead concentrate is insignificant. As an
illustration of this, the assays of 100 recent consecutive shipments of
lead ore from the district, taken at random, are cited as follows:
7 shipments assayed from 57 to 70% lead
15 shipments assayed from 70 to 75% lead
46 shipments assayed from 75 to 79% lead
32 shipments assayed from 80 to 84.4% lead
Average of 100 shipments 78.4% lead
Fourteen shipment samples, ranging from 70 to 84.4 per cent. lead, were
tested for zinc and iron. These averaged 2.24 per cent. Fe and 1.78
per cent. Zn, the highest zinc content being 4.5 per cent. No bismuth
or arsenic, and only very minute traces of antimony, have ever been
found in these ores. They contain only about 0.0005 per cent. of silver
(one-seventh of an ounce per ton) and scarcely more than that of copper
(occurring as chalcopyrite).
The pig lead produced from these ores is therefore very pure, soft and
uniform in quality, so that the term “soft Missouri lead” has become a
synonym for excellence in the manufacture of lead alloys and products,
such as litharge, red and white lead, and orange mineral. Its freedom
from bismuth, which is generally present in Colorado lead, makes it
particularly suitable for white lead; also for glass-maker’s litharge
and red lead. These oxides, for use in making crystal glass, must be
made by double refining so as to remove even the small quantities
of silver and copper that are present. The resulting product, made
from soft Missouri lead, is far superior to any refined lead produced
anywhere in this country or in Europe, even excelling the famous
Tarnowitz lead. It gives a luster and clarity to the glass that no
other lead will produce. Lead from southeastern Missouri, Kentucky,
Illinois, Iowa, and Wisconsin yields identical results, but the
refining is more difficult, not only because the lead contains a little
more silver and copper, but also because it contains more antimony.
The valuation of the lead concentrate produced in the Joplin district
is based upon a wet assay, usually the molybdate or ferrocyanide
method. The price paid is determined variously. One buyer pays a
fixed price for average ore, making no deductions; as, for example,
at present rates, $32.25 per 1000 lb. whether the ore assays 75 or 84
per cent. Pb, pig lead being worth $4.75 at St. Louis.[6] Another pays
$32.25 for 80 per cent. ore, or over, deducting 50c. per unit for ores
assaying under 80 per cent. Another pays for 90 per cent. of the lead
content of the ore as shown by the assay, at the St. Louis price of pig
lead, less a smelting charge of, say, $6 to $8 per ton of ore.
The history of the development of lead ore buying in the Joplin
district is rather curious. In the early days of the district the ore
was smelted wholly on Scotch hearths, which, with the purest ores,
would yield 70 per cent. metallic lead. No account was taken of the
lead in the rich slag, chemical determinations being something unknown
in the district at that time; it being supposed generally that pure
galena contained 700 lb. lead to the 1000 lb. of ore, the value of
700 lb. lead, less $4.50 per 1000 lb. of ore for freight and smelting
costs, was returned to the miner. The buyers graded the ore, according
to their judgment, by its appearance, as to its purity and also as to
its behavior in smelting; an ore, for example, from near the surface,
imbedded in the clay and coated more or less with sulphate, yielded its
metal more freely than the purer galenas from deeper workings.
This was the origin of the present method of buying—a system that would
hardly be tolerated except for the fact that the lead is, as previously
stated, considered a by-product of zinc mining.
Originally all the lead ore from the Missouri-Kansas district was
smelted in the same region, either in the air furnace (reverberatory
sweating-furnace) or in the water-back Scotch hearth. Competition
gradually developed in the market. Lead refiners found the pure
sulphide of special value in the production of oxidized products.
Some of the ore found its way to St. Louis, and even as far away as
Colorado, where it was used to collect silver. Since the formation of
the American Smelting and Refining Company and the greatly increased
output of the immense deposits of lead ore in Idaho, no Missouri lead
ore has gone to Colorado.
Up to 1901, one concern had more or less the control of the
southwestern Missouri ores. At the present time, lead ore is bought
for smelters in Joplin, Carterville, and Granby, Mo., Galena, Kan.,
and Collinsville, Ill., and complaint is heard that present prices are
really too high for the comfort of the smelters. Yet the old principle
of paying for lead ores upon the supposed yield of 70 per cent.,
irrespective of the real lead content, is still largely in vogue.
Any one interested in the matter will find it quite instructive to
calculate the returning charges, or gross profits, in smelting these
ores, on the basis of 70 per cent. recovery, at $32.25 per 1000 lb. of
ore, less 50c. per ton haulage, with lead at $4.77 per 100 lb. at St.
Louis. No deduction, it should be remarked, is ever made for moisture
in lead ores in this district. It is of interest to observe that
Dr. Isaac A. Hourwich estimates (in the U. S. Census Special Report
on Mines and Quarries recently issued) the average lead contents of
the soft lead ores of Missouri in 1902 at 68.2 per cent., taking as a
basis the returns from five leading mining and smelting companies of
Missouri, which reported a product of 70,491 tons of lead from 103,428
tons of their own and purchased ore. The average prices for lead ore
in 1902 were reported as follows, per 1000 lb.: Illinois, $19.53;
Iowa, $24.48; Kansas, $23.51; Missouri, $22.17; Wisconsin, $23.29;
Rocky Mountain and Atlantic Coast States, $10.90. In 1903, according
to Ingalls (“The Mineral Industry,” Vol. XII), the ore from the Joplin
district commanded an average price of $53 per 2000 lb., while the
average in the southeastern district was $46.81.
PART II
ROAST-REACTION SMELTING
SCOTCH HEARTHS AND REVERBERATORY FURNACES
LEAD SMELTING IN THE SCOTCH HEARTH
BY KENNETH W. M. MIDDLETON
(July 6, 1905)
In view of the fact that the Scotch hearth in its improved form is now
coming to the front again to some extent in lead smelting, it may prove
interesting to give a brief account of its present use in the north of
England.
Admitting that, where preliminary roasting is necessary, the best
results can be obtained with the water-jacketed blast furnace (this
being more especially the case where labor is an expensive item), we
have still as an alternative the method of smelting raw in the Scotch
hearth. At one works, which I recently visited, all the ore was smelted
raw; at another, all the ore received a preliminary roast, and it is
instructive to compare the results obtained in the two cases. The
following data refer to a fairly “free-smelting” galena assaying nearly
80 per cent. of lead.
When smelting raw ore in the hearth, fully 7½ long tons can be treated
in 24 hours, the amount of lead produced direct from the furnace in the
first fire being 8400 to 9000 lb.; this is equivalent to 56 to 60 per
cent. of lead, the remaining 24 to 20 per cent. going into the fume and
the slag.
When smelting ore which has received a preliminary roast of two hours,
12,000 lb. of lead is produced direct from the hearth, this being
equivalent to 65 per cent. of the ore. When the ore is roasted, the
output of the hearth is practically the same for all ores of equal
richness; but when smelting raw, if the galena is finely divided, the
output may fall much below that given herewith; while, on the other
hand, under the most favorable conditions it may rise to 12,000 lb. in
24 hours, or even more.
I had an opportunity of seeing a parcel of galena carrying 84 per cent.
of lead (but broken down very fine) smelted raw. The ore was kept damp
and the blast fairly low; but, in spite of that, a quantity of the ore
was blown into the flue, and only 5100 lb. of lead was produced from
the hearth in 24 hours.
Galena carrying only 65 per cent. of lead does not give nearly as
satisfactory results when smelted raw in the hearth; barely six tons of
ore can be smelted in 24 hours, and only 4500 to 5400 lb. of lead can
be produced directly. This is equivalent to, say, 43 per cent. of the
ore in the first fire; the remaining 22 per cent. goes into the slag or
to the flue as fume. Moreover, the 65 per cent. ore requires 1500 lb.
of coal in 24 hours, while the 80 per cent. galena uses only 1000 lb.
Turning now for a moment to the costs of smelting raw and of smelting
after a preliminary roast, we find that (in the case of the two works
we have been considering) the results are all in favor of smelting raw,
so far as a galena carrying nearly 80 per cent. is concerned.
The cost of smelting, per ton of lead produced, is given herewith:
ORE SMELTED RAW
Smelters’ wages $2.04
“ coal (425 lb.) 0.38
——-
Total $2.42
A very small quantity of lime is also used in this case for some ores,
but its cost would never amount to more than 4c. per ton of lead
produced.
ORE RECEIVING A PRELIMINARY ROAST
Roasters’ wages $0.61
“ coal (425 lb.) 0.65
Smelters’ wages 1.08
“ coal (75 lb.) 0.11
Peat and lime 0.08
——-
Total $2.53
It should be noted also that the smelters at the works where the ore
was not roasted receive higher pay. In the eight-hour shift they
produce about 1½ tons of lead; and as there are two of them to a
furnace, they make $3.06 between them, or $1.53 each. The two men
smelting roasted ore produce about two tons in an eight-hour shift, and
therefore each receives $1.08 per shift.
Coming now to fume-smelting in the hearth, we can again compare the
results obtained in smelting raw and after roasting. It is well to
bear in mind, also, that, while only 6½ per cent. of the lead goes in
the fume when smelting roasted ores in the hearth, a considerably
larger proportion is thus lost when smelting raw ores. When fume is
smelted raw, it is best dealt with when containing about 40 per cent.
of moisture. One man attends to the hearth (instead of two as when
smelting ore), and in 24 hours 3000 lb. of lead is produced, the amount
of coal used being 2100 lb. No lime is required.
When smelting roasted fume, two men attend to the hearth and the output
is 6000 lb. in 24 hours, the amount of coal used being 1800 lb. In this
latter case fluorspar happens to be available (practically free of
cost), and a little of it is used with advantage in fume-smelting, as
well as a small quantity of lime.
The cost of fume-smelting per ton of lead produced is given herewith:
FUME SMELTED RAW
Smelters’ wages $2.88
“ coal (1400 lb.) 2.13
——-—-
Total $5.01
FUME RECEIVING A PRELIMINARY ROAST
Roasters’ wages $2.08
“ coal (1450 lb.) 2.18
Smelters’ wages 2.04
“ coal (600 lb.) 0.92
Peat and lime 0.08
———--
Total $7.30
In this case, as in that of ore, the smelter of the raw fume gets
better pay; he has $1.44 per eight-hour shift, while the smelter of the
roasted ore has only $1.02 per eight-hour shift.
Fume takes four hours to roast, as compared to the two hours taken by
ore.
From these facts regarding Scotch-hearth smelting, it would seem that
with galena carrying, say, over 70 per cent. lead (but more especially
with ore up to 80 per cent. in lead, and, moreover, fairly free from
impurities detrimental to “free” smelting), very satisfactory results
can be obtained by smelting raw. Against this, however, it must be said
that at the works where the ore is roasted attempts at smelting raw
have been made several times without sufficient success to justify the
adoption of this method, although the ores smelted average 75 per cent.
lead and seem quite suitable for the purpose.
Probably this may be accounted for by the fact that the method of
running the furnace when raw ore is being smelted is rather different
from that adopted when dealing with roasted ore. Moreover, at the works
under notice the furnaces are not of the most modern construction; and,
as the old custom of dropping a peat in front of the blast every time
the fire is made up still survives, it is necessary to shut off the
blast while this is being done, and the fire is then apt to get rather
slack.
The gray slag produced in the hearth is smelted in a small blast
furnace, a little poor fume, and sometimes a small quantity of
fluorspar, being added to facilitate the process. Some figures
regarding slag-smelting may be of interest. The slag-smelters produce
9000 lb. of lead in 24 hours. The cost of slag-smelting per ton of lead
produced is as follows:
Smelters’ wages $1.60
Coke (1500 lb.) 3.42
Peat 0.06
———--
Total $5.08
Recent analyses of Weardale (Durham county) lead smelted in the Scotch
hearth, and slag-lead smelted in the blast furnace, are given herewith:
─────────┬───────────────────┬────────────────────┬──────────────────
│ FUME-LEAD FROM │ SILVER-LEAD FROM │ SLAG-LEAD FROM
│ HEARTH │ HEARTH │ BLAST FURNACE
─────────┼───────────────────┼────────────────────┼──────────────────
Lead │ 99.957 │ 99.957 │ 99.013
Silver │ 0.0035 │ 0.0200 │ 0.0142
│ (1oz. 2dwt. 21gr. │ (6oz. 10dwt. 16gr. │(4oz. 12dwt. 18gr.
│ per Long Ton) │ per Long Ton) │ per Long Ton)
Tin │ nil │ nil │ nil
Antimony │ nil │ nil │ 0.874
Copper │ nil │ nil │ 0.024
Iron │ 0.019 │ 0.019 │ 0.023
Zinc │ nil │ nil │ nil
│ ──────── │ ──────── │ ────────
│ 99.9795 │ 99.9960 │ 99.9482
─────────┴───────────────────┴────────────────────┴──────────────────
The ordinary form of the Scotch hearth is probably too well known
to need much description. The dimensions which have been found most
suitable are as follows: Front to back, 21 in.; width, 27 in.; depth
of hearth, 8 to 12 in. Formerly the distance from front to back was 24
in., but this was found too much for the blast and for the men.
The cast-iron hearth which holds the molten lead is set in brickwork;
if 8 in. deep and capable of holding about ¾ ton of lead, it is quite
large enough. The workstone or inclined plate in front of the hearth
is cast in one piece with it, and has a raised holder on either side
at the lower edge, and a gutter to convey the overflowing lead to the
melting-pot. The latter is best made with a partition and an opening
at the bottom through which clean lead can run, so that it can be
ladled into molds without the necessity for skimming the dross off
the surface. It is well also to have a small fireplace below the
melting-pot.
On each side of the hearth, and resting on it, is a heavy cast-iron
block, 9 in. thick, 15 in. high, 27 to 28 in. long. To save metal,
these are now cast hollow and air is caused to pass through them. On
the back of the hearth stands another cast-iron block known as the
“pipestone,” through which the blast comes into the furnace. In the
older forms of pipestone the blast comes in through a simple round or
oval pipe, a common size being 3 or 4 in. wide by 2½ in. high, and the
pipestone is not water-cooled. With this construction the hearth will
not run satisfactorily unless the pipestone is set with the greatest
care, so as to have the tuyere exactly in the center, and as there
is no water-cooling the metal quickly burns away when fume is being
smelted. Moreover, the blast is apt to be stopped by slag adhering to
the end of the pipe. As already mentioned, a peat is dropped in front
of the blast every time the fire is made up, with the object of keeping
a clear passage open for the blast. This old custom has, however,
several serious disadvantages; first, it prevents the blast being kept
on continuously; and, second, it makes it necessary to have the hearth
open at the top so that the smelter-man can go in by the side of it. In
this case the ore is fed from the side by the smelter-man, who works
under the large hood placed above the furnace to carry away the fume.
Even when he is engaged in shoveling back the fire from the front and
is not underneath the hood, it is impossible to prevent some fume from
blowing out; and there is much more liability to lead-poisoning than
when the hearth is closed at the top by the chimney and the smelter-men
work from the front. The best arrangement is to have the hearth
entirely closed in by the chimney, except for the opening at the front,
and to have a small auxiliary flue above the workstone leading direct
to the open air to catch any fume that may blow out past the shutter in
front of the hearth.
In an improved form of pipestone, a pipe connected to the blast-main
fits into the semicircular opening at the back and is driven tight
against a ridge in the flat side of the opening. Going through the
pipestone, the arch becomes gradually flatter, and the blast emerges
into the hearth, about 2 in. above the level of the molten lead,
through an oblong slit 12 in. long by 1 in. wide, with a ledge
projecting 1½ in. immediately above it. The back and front are similar,
so that when one side gets damaged the pipestone can be turned back to
front.
Water is conveyed in a 2½ in. iron pipe to the pipestone, and after
passing through it is led away from the other end to a water-box, which
stands beside the hearth and into which the red-hot lumps of slag are
thrown to safeguard the smelters from the noxious fumes.
On the top of the pipestone rests an upper backstone, also of cast
iron; it extends somewhat higher than the blocks at the sides. All this
metal above the level of the lead is necessary because the partially
fused lumps which stick to it have to be knocked off with a long bar,
so that if fire-bricks were used in place of cast iron they would soon
be broken up and destroyed.
With a covered-in hearth, when the ore is charged from the front,
the following is the method adopted in smelting raw ore: The charge
floats on the molten lead in the hearth, and at short intervals the
two smelters running the furnace ease it up with long bars, which they
insert underneath in the lead. Any pieces of slag adhering to the sides
and pipestone are broken off. After easing up the fire, the lumps of
partially reduced ore, mixed with cinders and slag, are shoveled on
to the back of the fire; the slag is drawn out upon the workstone
(any pieces of ore adhering to it being broken off and returned to
the hearth), and it is then quenched in a water-box placed alongside
the workstone. One or two shovelfuls of coal, broken fairly small
and generally kept damp, are thrown on the fire, together with the
necessary amount of ore, which is also kept damp if in a fine state
of division. It is part of the duty of the two smelters to ladle out
the lead from the melting-pot into the molds. In smelting ore a fairly
strong, steady blast is required, and it is made to blow right through
so as to keep the front of the fire bright. A little lime is thrown on
the front of the fire when the slag gets too greasy.
When smelting raw fume one man attends to the furnace. It does not
have to be made up nearly as frequently, the work being easier for
one man than smelting ore is for two. The unreduced clinkers and slag
are dealt with exactly as in smelting ore; and coal is also, in this
case, thrown on the back of the fire, but the blast does not blow
right through to the front. On the contrary, the front of the fire is
kept tamped up with fume, which should be of the coherency of a thick
mud. The blast is not so strong as that necessary for ore. The idea is
partially to bake the fume before submitting it to the hottest part of
the furnace, or to the part where the blast is most strongly felt. It
is only when smelting fume that it is necessary to keep the pipestone
water-cooled.
To start a furnace takes from two to three hours. The hearth is left
full of lead, and this has to be melted before the hearth is in normal
working order. Drawing the fire takes about three-quarters of an hour;
the clinkers are taken off and kept for starting the next run, and the
sides and back of the hearth are cleaned down.
THE FEDERAL SMELTING WORKS, NEAR ALTON, ILL.[7]
BY O. PUFAHL
(June 2, 1906)
The works of the Federal Lead Company, near Alton, Ill., were erected
in 1902. They have a connection with the Chicago, Peoria & St. Louis
Railway, by which they receive all their raw materials, and by which
all the lead produced is shipped.
The ore smelted is galena, with dolomitic gangue, and a small quantity
of pyrites (containing a little copper, nickel, and cobalt) from
southeastern Missouri, and consists chiefly of fine concentrates,
containing 60 to 70 per cent. lead. In addition thereto a small
proportion of lump ore is also smelted.
A striking feature at these works is the excellent facility for
handling the materials. The bins for the ore, coke and coal are made
of concrete and steel and are filled from cars running on tracks
laid above them. For transporting the materials about the works a
narrow-gage railway with electric locomotives is used.
The ores are smelted by the Scotch-hearth process. There are 20 hearths
arranged in a row in a building constructed wholly of steel and stone.
The sump (4 × 2 × 1 ft.) of each furnace contains about one ton of
lead. The furnaces are operated with low-pressure blast from a main
which passes along the whole row. The blast enters the furnace from a
wind chest at the back through eight 1 in. iron pipes, 2 in. above the
bath of lead. The two sides and the rear wall are cooled by a cast-iron
water jacket of 1 in. internal width.
Two men work, in eight-hour shifts, at each of the furnaces, receiving
4.75 and 4.25c. respectively for every 100 lb. of lead produced. The
ore is weighed out and heaped up in front of the furnaces; on the
track near by the coke is wheeled up in a flat iron car with two
compartments. The furnacemen are chiefly negroes. At the side of each
furnace is a small stock of coal, which is used chiefly for maintaining
a small fire under the lead kettle. Only small quantities of coal are
added from time to time during the smelting operation.
Over each furnace is placed an iron hood, through which the fumes and
gases escape. They pass first through a collecting pipe, extending
through the whole works, to a 1500 ft. dust flue, measuring 10 × 10
ft., in internal cross-section. Near the middle of this is placed a
fan of 100,000 cu. ft. capacity per minute, which forces the fumes and
gases into the bag-house, where they are filtered through 1500 sacks of
loosely woven cotton cloth, each 25 ft. long and 18 in. in diameter,
and thence pass up a 150 ft. stack.
The dust recovered in the collecting flue is burnt, together with the
fume caught by the bags, the coal which it contains furnishing the
combustible. It burns smolderingly and frits together somewhat. The
product (chiefly lead sulphate) is then smelted in a shaft furnace,
together with the gray slag from the hearth furnaces. The total
extraction of lead is about 98 per cent., i.e., the combined process
of Scotch-hearth and blast-furnace smelting yields 98 per cent. of the
lead contained in the crude ore.
The direct yield of lead from the Scotch hearths is about 70 per cent.
They also produce gray slag, containing much lead, which amounts to
about 25 per cent. of the weight of the ore. About equal proportions
of lead pass into the slag and into the flue dust. When working to
the full capacity, with rich ore (80 per cent. lead and more) the 20
furnaces can produce about 200 tons of lead in 24 hours. The coke
consumption in the hearth furnaces amounts to only 8 per cent. of the
ore. The lead from these furnaces is refined for 30 minutes to one
hour by steam in a cast-iron kettle of 35 tons capacity, and is cast
into bars either alone or mixed with lead from the shaft furnace. The
“Federal Brand” carries nearly 99.9 per cent. lead, 0.05 to 0.1 per
cent. copper, and traces of nickel and cobalt.
The working up of the between products from the hearth-furnaces is
carried out as follows: Slag, burnt flue dust and roasted matte from
a previous run, together with a liberal proportion of iron slag (from
the iron works at Alton), are smelted in a 12-tuyere blast furnace
for work-lead and matte. The furnace is provided with a lead well at
the back. The matte and slag are tapped off together at the front and
flow through a number of slag pots for separation. The shells which
remain adhering to the walls of the pots on pouring out the slag are
returned to the furnace. All the waste slag (containing about 0.5 per
cent. lead) is dumped down a ravine belonging to the territory of the
smeltery.
The lead from the shaft furnace is liquated in a small reverberatory
furnace, of which the hearth consists of two inclined perforated
iron plates. The residue is returned to the shaft furnace, while the
liquated lead flows directly to the refining kettle, which is filled
in the course of four hours. Here it is steamed for about one hour and
is then cast into bars through a Steitz siphon, after skimming off the
oxide. The matte is crushed and roasted in a reverberatory furnace (60
ft. long).
The power plant comprises three Stirling boilers and two 250 h. p.
compound engines, of which one is for reserve; also one steam-driven
dynamo, coupled direct to the engine, furnishing the current for the
entire plant, for the electric locomotives, etc.
The coke is obtained from Pennsylvania and costs about $4 a ton, while
the coal comes from near-by collieries and costs $1 per ton.
In the well-equipped laboratory the lead in the ores and slags is
determined daily by Alexander’s (molybdate) method, while the silver
content of the lead (a little over 1 oz. per ton) is estimated only
once a month in an average sample. When the plant is in full operation
it gives employment to 150 men. Cases of lead-poisoning are said to
occur but rarely, and then only in a mild form.
LEAD SMELTING AT TARNOWITZ
(September 23, 1905)
The account of the introduction of the Huntington-Heberlein process at
Tarnowitz, Prussia, published elsewhere in this issue, is of peculiar
interest inasmuch as it tells of the complete displacement by the new
process of one of the old processes of lead smelting which had become
classic in the art. The roast-reaction process of lead smelting,
especially as carried out in reverberatory furnaces, has been for a
long time decadent, even in Europe. Tarnowitz was one of the places
where it survived most vigorously.
Outside of Europe, this process never found any generally extensive
application. It was tried in the Joplin district, and elsewhere in
Missouri, with Flintshire furnaces in the seventies. Later it was
employed with modified Flintshire and Tarnowitz furnaces at Desloge,
in the Flat River district of Missouri, where the plant is still in
operation, but on a reduced scale.
The roast-reaction process of smelting, as practised at Tarnowitz,
was characterized by a comparatively large charge, slow roasting and
low temperature, differing in these respects from the Carinthian and
Welsh processes. It was not aimed to extract the maximum proportion of
lead in the reverberatory furnace itself, the residue therefrom, which
inevitably is high in lead, being subsequently smelted in the blast
furnace. Ores too low in lead to be suitable for the reverberatory
smelting were sintered in ordinary furnaces and smelted in the blast
furnace together with the residue from the other process. In both of
these processes the loss of lead was comparatively high. One of the
most obvious advantages of the Huntington-Heberlein process is its
ability to reduce the loss of lead. The result in that respect at
Tarnowitz is clearly stated by Mr. Biernbaum, whose paper will surely
attract a good deal of attention.[8]
LEAD SMELTING IN REVERBERATORY FURNACES AT DESLOGE, MO.
BY WALTER RENTON INGALLS
(December 16, 1905)
The roast-reaction method of lead smelting in reverberatory furnaces
never found any general employment in the United States, although
in connection with the rude air-furnaces it was early introduced in
Missouri. The more elaborate Flintshire furnaces were tried at Granby,
in the Joplin district, but they were displaced there by Scotch
hearths. The most extensive installation of furnaces of the Flintshire
type was made at Desloge, in the Flat River district of southeastern
Missouri. This continued in full operation until 1903, when the major
portion of the plant was closed, it being found more economical to ship
the ore elsewhere for smelting. However, two furnaces have been kept
in use to work up surplus ore. As a matter of historic interest, it is
worth while to record the technical results at Desloge, which have not
previously been described in metallurgical literature.
The Desloge plant, which was situated close to the dressing works
connected with the mine, and was designed for the smelting of its
concentrate, comprised five furnaces. The furnaces were of various
constructions. The oldest of them was of the Flintshire type, and
had a hearth 10 ft. wide and 14 ft. long. The other furnaces were a
combination of the Flintshire and Tarnowitz types. They were built
originally like the newer furnaces at Tarnowitz, Upper Silesia, with a
rather large rectangular hearth and a lead sump placed at one side of
the hearth near the throat end; but good results were not obtained from
that construction, wherefore the furnaces were rearranged with the sump
at one side, but in the middle of the furnace, as in the Flintshire
form. The rectangular shape of the Tarnowitz hearth was, however,
retained. Furnaces thus modified had hearths 11 ft. wide and 16 ft.
long, except one which had a hearth 13 ft. wide.
The same quantity of ore was put through each of these furnaces, the
increase in hearth area being practically of no useful effect, because
of inability to attain the requisite temperature in all parts of the
larger hearths with the method of heating employed. The men objected
especially to a furnace with hearth 13 ft. wide, which it was found
difficult to keep in proper condition, and also difficult to handle
efficiently. Even the width of 11 ft. was considered too great, and
preference was expressed for a 10 ft. width. In this connection, it may
be noted that the old furnaces at Tarnowitz were 11 ft. 9 in. long and
10 ft. 10 in. wide, while the new furnaces were 16 ft. long and 8 ft.
10 in. wide (Hofman, “Metallurgy of Lead,” fifth edition, p. 112). All
of these dimensions were exceeded at Desloge.
The Flintshire furnaces at Desloge had three working doors per side;
the others had four, but only three per side were used, the doors
nearest the throat end being kept closed because of insufficient
temperature in that part of the furnace. The furnace with hearth 11
× 14 ft. had a grate area of 6.5 × 3 ft. = 19.5 sq. ft.; the 11 × 16
furnaces had grates 8 × 3 = 24 ft. sq. The ratios of grate to hearth
area were therefore approximately 1:8 and 1:7.3, respectively. (Compare
with ratio of 1:10 at Tarnowitz, and 1:6⅔ at Stiperstones.) The ash
pits were open from behind in the customary English fashion. The grate
bars were cast iron, 36 in. long. The bars were 1 in. thick at the top,
with ⅝ in. spaces between them. The open spaces were 32 in. long,
including the rib in the middle. The bars were 4 in. deep at the middle
and 2 in. at the ends. The distance from the surface of the grate bars
to the fire-door varied in the different furnaces. Some of those with
hearths 11 × 16 ft. and grates 8 × 3 ft. had the bars 6 in. below the
fire-door; in others the bars were almost on a level with the fire-door.
The furnaces were run with a comparatively thin bed of coal on the
grate, and combustion was very imperfect, the percentage of unburned
carbon in the ash being commonly high. This was unavoidable with the
method of firing employed and the inferior character of the coal
(southern Illinois). The excessive consumption of coal was due largely,
however, to the practice of raking out the entire bed of coal at the
beginning of the operation of “firing down” (beginning the reaction
period), when a fresh fire was built with cordwood and large lumps of
coal.
Each furnace had two flues at the throat, 16 × 18 in. in size, each
flue being provided with a separate damper. Each furnace had an
iron chimney approximately 55 ft. high, of which 13 ft. was a brick
pedestal (64 × 64 in.) and the remaining 42 ft. sheet steel, guyed. The
chimneys were 42 in. in diameter. The distance from the outside end
of the furnace to the chimney was approximately 6 ft., and there was
consequently but little opportunity for flue dust to collect in the
flue. About once a month, however, the chimney was opened at the base
and about two wheelbarrows (say 600 lb.) of flue dust, assaying about
50 per cent. lead, was recovered per furnace.
The furnace house was a frame building 45 ft. wide, with boarded sides
and a corrugated-iron pitch roof, supported by steel trusses. The
furnaces were set in this house, side by side, their longitudinal axes
being at right angles to the longitudinal axis of the building. The
distance from the outside of the fire-box end of the furnace to the
side of the building was 10 ft. The coal was unloaded from a railway
track alongside of the building and was wheeled to the furnace in
barrows. Some of the furnaces were placed 18 ft. apart; others 22 ft.
apart. The men much preferred the greater distance, which made their
work easier, an important consideration in this method of smelting.
The hight from the floor to the working door of the furnace was
approximately 36 in. The working doors were formed with cast-iron
frames, making openings 7 × 11 in. on the inside and 15 × 28 in. on
the outside. On the side of the furnace opposite the middle working
door was placed a cast-iron hemispherical pot, set partially below the
floor-line. This pot was 16 in. deep and 24 in. in diameter; the metal
was ¼ in. thick. The distance from the top of the pot to the line of
the working door was 31 in.; from the top of the pot to the bottom of
the tap-door was 7 in. The tap-door was 4 in. wide and 9 in. high,
opening through a cast-iron plate 1½ in. thick. Below the tap-door
and on a line with the upper rim of the pot was a tap-hole 3½ in. in
diameter. The frames of the working doors had lugs in front, against
which the buckstaves bore, to hold the frames in position. All other
parts of the sides of the furnace, including the fire-box, were cased
with ⅝ in. cast-iron plates, which were obviously too light, being
badly cracked.
The cost of a furnace when built in 1893 was approximately $1400,
not including the chimney; but with the increased cost of material
the present expense would probably be about $2000. Notwithstanding
the light construction of the furnaces, repairs were never a large
item. Once a month a furnace was idle about 24 hours while the throat
was being cleaned out, and every two months some repairing, such as
relining the fire-boxes, etc., was required. If repairs had to be made
on the inside of the furnace, two days would be lost while it was
cooling sufficiently for the men to enter. In refiring a furnace, from
8 to 12 hours was required to raise it to the proper temperature. Out
of the 365 days of the year, a furnace would lose from 20 to 25 days,
for cleaning the throat and making repairs to the fire-box, arch, etc.
When a furnace was run with two shifts the schedule of operation was as
follows:
Drop charge 4 a.m.
Begin work 7 a.m.
Begin firing down 11 a.m.
Begin first tapping 1 p.m.
Rake out slag 2.30 p.m.
Begin second tapping 3 p.m.
Drop charge 4 p.m.
Begin working 5.30 p.m.
Begin firing down 11 p.m.
Begin first tapping 1 a.m.
Rake out slag 2.30 a.m.
Begin second tapping 3 p.m.
With three shifts on a furnace, the schedule was as follows:
Drop charge 7 a.m.
Begin firing down 12 a.m.
Begin tapping 1 p.m.
Rake out slag 2 p.m.
Begin tapping 2.30 p.m.
Drop charge 3 p.m.
Begin firing down 8 p.m.
Begin tapping 9 p.m.
Rake out slag 10 p.m.
Begin tapping 10.30 p.m.
Drop charge 11.00 p.m.
Begin firing down 4 a.m.
Begin tapping 5 a.m.
Rake out slag 6 a.m.
Begin tapping 6.30 a.m.
The hearths were composed of about 8 in. of gray slag beaten down
solidly on a basin of brick, which rested on a filling of clay, rammed
solid. The hearth was patched if necessary after the drawing of each
charge.
The system of smelting was analogous to that which was practiced
in Wales rather than to the Silesian, the charges being worked off
quickly, and with the aim of making a high extraction of lead directly
and a gray slag of comparatively low content in lead. The average
furnace charge was 3500 lb. At the beginning of the reaction period
about 85 to 100 lb. of crushed fluorspar was thrown into the furnace
and mixed well with the charge. The furnace doors were then closed
tightly and the temperature raised, the grate having previously been
cleaned. At the first tapping about 1200 lb. of lead would be obtained.
A small quantity of chips and bark was thrown into the lead in the
kettle, which was then poled for a few minutes, skimmed, and ladled
into molds, the pigs weighing 80 lb. The skimmings and dross were
put back into the furnace. The pig lead was sold as “ordinary soft
Missouri.” The gray slag was raked out of the furnace, at the end of
the operation, into a barrow, by which it was wheeled to a pile outside
of the building. Shipments of the slag were made to other smelters from
time to time, 95 per cent. of its lead content being paid for when its
assay was over 40 per cent., and 90 per cent. when lower.
Each furnace was manned by one smelter ($1.75) and one helper ($1.55)
per shift, when two shifts per 24 hours were run. They had to get their
own coal, ore and flux, and wheel away their gray slag and ashes. In
winter, when three shifts were run, the men were paid only $1.65 and
$1.50 respectively. There was a foreman on the day shift, but none at
night. The total coal consumption was ordinarily about 0.8 to 0.9 per
ton of ore. Run-of-mine coal was used, which cost about $2 per ton
delivered. The coal was of inferior quality, and it was wastefully
burned, as previously referred to, wherefore the consumption was high
in comparison with the average at Tarnowitz, where it used to be about
0.5 per ton of ore.
The chief features of the practice at Desloge are compared with those
at Tarnowitz, Silesia and Holywell (Flintshire), and Stiperstones
(Shropshire), Wales, in the following table, the data for Silesia and
Wales being taken from Hofman’s “Metallurgy of Lead,” fifth edition,
pp. 112, 113.
──────────────────────┬─────────┬────────┬─────────┬─────────┬────────
DETAIL │HOLYWELL │ STIPER-│TARNOWITZ│TARNOWITZ│ DESLOGE
│ │ STONES │ │ │
──────────────────────┼─────────┼────────┼─────────┼─────────┼────────
Hearth length, ft. │ 12.00 │ 9.75 │ 11.75 │ 16.00 │ 16.00
Hearth width, ft. │ 9.50 │ 9.50 │ 10.83 │ 8.83 │ 11.00
Grate length, ft. │ 4.50 │ 4.50 │ 8.00 │ 8.00 │ 8.00
Grate width, ft. │ 2.50 │ 2.50 │ 1.67 │ 1.67 │ 3.00
Grate area: hearth │ │ │ │ │
area │ 1:8 │ 1:6⅔ │ 1:10 │ 1:10 │ 1:7⅓
Charges per 24 hr., │ 3 │ 3 │ 2 │ 2 │ 3
Ore smelted per │ │ │ │ │
24 hr., lb. │ 7,050 │ 7,050 │ 8,800 │ 16,500 │ 10,500
Assay of ore, % Pb │ 75-80 │ 77.5 │ 70-74 │ 70-74 │ 70
Gray slag, % of charge│ 12 │ │ 15 │ 30 │ 27
Gray slag, % Pb │ 55 │ │ 38.8 │ 56 │ 38
Men per 24 hr. │ 6 │ 4 │ 4 │ 6 │ 6
Coal used per ton ore │0.57-0.76│ 0.56 │ 0.46 │ 0.50 │ 0.90
──────────────────────┴─────────┴────────┴─────────┴─────────┴────────
The regular furnace charge at Desloge was 3500 lb. The working of three
charges per 24 hours gave a daily capacity of 10,500 lb. per furnace.
These figures refer to the wet weight of the concentrate, which was
smelted just as delivered from the mill. Its size was 9 mm. and finer.
Assuming its average moisture content to be 5 per cent., the daily
capacity per furnace was about 10,000 lb. (5 tons) of dry ore.
The metallurgical result is indicated by the figures for two months
of operation in 1900. The quantity of ore smelted was 1012 tons,
equivalent to approximately 962 tons dry weight. The pig lead produced
was 523.3 tons, or 54.4 per cent. of the weight of the ore. The gray
slag produced was 262.25 tons, or about 27 per cent. of the weight of
the ore. The assay of the ore was approximately 70 per cent. lead,
giving a content of 673.4 tons in the ore smelted. The gray slag
assayed approximately 38 per cent. lead, giving a content of 99.66
tons. Assuming that 90 per cent. of the lead in the gray slag be
recoverable in the subsequent smelting in the blast furnace, or 89.7
tons, the total extraction of lead in the process was 523.3 + 89.7 ÷
673.4 = 91 per cent. The metallurgical efficiency of the process was,
therefore, reasonably high, especially in view of the absence of dust
chambers.
* * * * *
The cost of smelting with five furnaces in operation, each treating
three charges per day, was approximately as follows:
1 foreman at $3 $3.00
5 furnace crews at $9.90 49.50
Unloading 21 tons of coal at 6c. 1.26
Loading 14 tons lead at 15c. 2.10
“ 7 tons gray slag at 15c. 1.05
——————
Total labor $56.91
21 tons coal at $2 $42.00
Flux and supplies 13.00
Blacksmithing and repairs 10.00
——————
Total $121.91
On the basis of 6.25 tons of wet ore, this would be $4.65 per ton. The
actual cost in seven consecutive months of 1900 was as follows: Labor,
$1.98 per ton; coal, $1.86; flux and supplies, $0.51; blacksmithing and
repairs, $0.39; miscellaneous, $0,017; total, $4.757. If the cost of
smelting the gray slag be reckoned at $8 per ton, and the proportion
of gray slag be reckoned at 0.25 ton per ton of galena concentrate,
the total cost of treatment of the latter comes to about $6.75 per ton
of wet charge, or about $7 per ton of dry charge. This cost could be
materially reduced in a larger and more perfectly designed plant.
The practice at Desloge did not compare unfavorably, either in respect
to metal extracted or in smelting cost, with the roast-reduction method
of smelting or the Scotch hearth method, as carried out in the plants
of similar capacity and approximately the same date of construction,
smelting the same class of ore, but the larger and more recent plants
in the vicinity of St. Louis could offer sufficiently better terms to
make it advisable to close down the Desloge plant and ship the ore to
them. One of the drawbacks of the reverberatory method of smelting
was the necessity of shipping away the gray slag, the quantity of
that product made in a small plant being insufficient to warrant the
operation of an independent shaft furnace.
PART III
SINTERING AND BRIQUETTING
THE DESULPHURIZATION OF SLIMES BY HEAP ROASTING AT BROKEN HILL[9]
BY E. J. HORWOOD
(August 22, 1903)
It is well known that, owing to the intimate mixture of the
constituents of the Broken Hill sulphide ores, a great deal of crushing
and grinding is required to detach the particles of galena from the
zinc blende and the gangue; and it will be understood, therefore, that
a considerable amount of the material is converted into a slime which
consists of minute but well-defined particles of all the constituents
of the ore, the relative proportions of which depend on the dual
characteristics of hardness and abundance of the various constituents.
An analysis of the slime shows the contents to be as follows;
Galena (PbS) 24.00
Blende (ZnS) 29.00
Pyrite (FeS₂) 3.38
Ferric oxide (Fe₂O₃) 4.17
Ferrous oxide (FeO) contained in garnets 1.03
Oxide of manganese (MnO) contained in rhodonite and garnets 6.66
Alumina (Al₂O₃) contained in kaolin and garnets 5.40
Lime (CaO) contained in garnets, etc. 3.40
Silica (SiO₂) 22.98
Silver (Ag) .06
——————
100.48
Galena, being the softest of these, is found in the slimes to a larger
extent than in the crude ore; it is also, for the same reason, in the
finest state of subdivision, as is well illustrated by the fact that
the last slime to settle in water is invariably much the richest in
lead, while the percentages of the harder constituents, zinc blende and
gangue, show a corresponding reduction in quantity, by reason of their
being generally in larger sized particles and consequently settling
earlier.
The fairly complete liberation of each of the constituent minerals
of the ore that takes place in sliming tends, of course, to help
the production of a high-grade concentrate by the use of tables and
vanners, and undoubtedly a fair recovery of lead is quite possible,
even with existing machines, in the treatment of fine slimes; but,
owing to the great reduction in the capacity of the machines, which
takes place when it is attempted to carry the vanning of the finer
slimes too far, and the consequently greatly increased area of the
machines that would be necessary, the operation, sooner or later,
becomes unprofitable.
The extent to which the vanner treatment of slimes should be carried
is, of course, less in the case of those mines owning smelters than
with those which have to depend on the sale of concentrates as their
sole source of profit. In the case of the Proprietary Company,
all slime produced in crushing is passed over the machines after
classification. A high recovery of lead in the form of concentrates
is, of course, neither expected nor obtained, for reasons already
explained; but the finest lead-bearing slimes are allowed to unite
with the tailings, which are collected from groups of machines, and
are then run into pointed boxes, where, with the aid of hydraulic
classification, the fine rich slimes are washed out and carried to
settling bins and tanks, where the water is stilled and allowed to
deposit its slime, and pass over a wide overflow as clear water. The
slime thus recovered amounts to over 1200 tons weekly, or about 11 per
cent., by weight, of the ore, and assays about 20 per cent. lead, 17
per cent. zinc, and 18 oz. silver, and represents, in lead value, about
11 per cent. of the original lead contents of the crude ore and rather
more than that percentage in silver contents. These slimes are thus a
by-product of the mills, and their production is unavoidable; but as
they are not chargeable with the cost of milling, they are an asset of
considerable value, more especially so since it has been demonstrated
that they can be desulphurized sufficiently for smelting purposes by a
simple operation, and, at the same time, converted into such a physical
condition as renders the material well suited for smelting, owing to
its ability to resist pressure in the furnaces.
The Broken Hill Proprietary Company has many thousands of tons of
these slimes which the smelters have hitherto been unable to cope with,
owing to the roasters being fully occupied with the more valuable
concentrates. Moreover, the desulphurization of slimes in Ropp
mechanical roasters is objectionable for various reasons, namely, owing
to the large amount of dust created with such fine material, resulting
injuriously to the men employed; also on account of the reduction in
the capacity of the roasters, and consequent increase in working cost,
owing to the lightness of the slime, especially when hot, as compared
with concentrates, and the necessity for limiting the thickness of
material on the bed of the roasters to a certain small maximum.
Further, the desulphurization of the slimes is no more complete with
the mechanical roasters than in the case of heap roasting, and the
combined cost of roasting and briquetting being quite three shillings
(or 75c.) per ton in excess of the cost of heap roasting, the
latter possesses many advantages. These heaps are being dealt with,
preparatory to roasting, by picking down the material in lumps of about
5 in. in thickness, while the fine dry smalls, unavoidably produced,
are worked up in a pug mill with water, and dealt with in the same way
as the wet slime produced from current work.
The slime, as produced by the mills, is run from bins into railway
trucks in a semi-fluid condition, and shortly after being tipped
alongside one of the various sidings on the mine is in a fit condition
to be cut with shovels into rough bricks, which dry with fair rapidity,
and when required for roasting are easily reloaded into railway trucks.
As each man can cut about 20 tons of bricks per day, the cost is small.
Various other methods of lumping the slime were tried, including
trucking the semi-fluid material on movable trams, alongside which were
set laths, about 9 in. apart, which enabled long slabs to be formed
9 in. wide and 5 in. thick, which were, after drying, picked up in
suitable lumps and loaded in platform trucks, thence on railway trucks.
Owing to the inferior roasting that takes place with bricks having flat
sides, which are liable to come into close contact in roasting, and
to the rather high labor cost, this method was discontinued. Another
method was to allow the slime to dry partially after being emptied
from railway trucks, and to break it into lumps by means of picks;
but this method entailed the making of an increased amount of smalls,
besides taking up more siding room, owing to the extra time required
for drying, as compared with the method now in use. Ordinary bricking
machines could, of course, be used, but when the cost of handling the
slime before and after bricking is counted, the cost would be greater
than with the simple method now in use; the material being in too
fluid a condition for making into bricks until some time elapses for
drying, a double handling would be necessitated before sending it to
the bricking machine. If, however, the slime could be allowed time to
dry sufficiently in the trucks, bricking by machinery would probably be
preferable. Rather more than 10 per cent. of smalls is made in handling
the lumps in and out of the railway trucks, and this is, as already
noted, worked up with water in a pug mill at the sintering works, and
used partly for covering the heaps with slime to exclude an excessive
amount of air. The balance is thrown out and cut into bricks, as
already described.
At the heaps the lumps are at present being thrown from one man to
another to reach their destination in the heap, but the sidings have
been laid out in duplicate with a view to enabling traveling cranes to
be used on the line next the heap, the lumps to be loaded primarily
into wooden skips fitting the trucks. It is probable, however, that
the lumps will require to be handled out of the skips into their place
in the heap, as the brittle nature of the material may be found to
render automatic tipping impracticable. A considerable saving in labor
would nevertheless accompany the use of cranes, which would likewise be
advantageous in loading the sintered material.
In order to reduce the inconvenience arising from fumes, length is very
desirable in siding accommodation, so that heap building may be carried
on at a sufficient distance from the burning kilns. It is for the same
reason preferable to build in a large tonnage at one time, lighting
the heaps altogether. As the heaps burn about two weeks only, long
intervals intervene, during which the fumes are absent.
In the experimental stages of slime roasting, fuel, chiefly wood, was
used in quantities up to 5 per cent., and was placed on the ground at
the bottom of the heap, where also a number of flues, loosely built
bricks, were placed for the circulation of air. The amount of fuel
used has, however, been gradually reduced, until the present practice
of placing no fuel whatever in the bottom was arrived at; but instead
less than 1 per cent. of wood is now burned in small enlargements of
the flues, under the outer portion of the pile, and placed about 12
ft. apart at the centers. This is found to be sufficient to start the
roasting operation within 24 hours of lighting, after which no further
fuel is necessary.
As regards the dimensions of the heaps, the width found most suitable
is 22 ft. at the base, the sides sloping up rather flatter than one to
one, with a flat section on top reaching about 7 ft. in hight. As there
is always about 6 in. of the outer crust imperfectly roasted, it is
advisable to make the length as great as possible, thus minimizing the
surface exposed. The company is building heaps up to 2000 ft. long.
During roasting care is required to regulate the air supply, the object
being to avoid too fierce a roast, which tends to sinter and partially
fuse the material on the outer portions of the lumps, while inside
there is raw slime. By extending the roast over a longer period this is
avoided, and a more complete desulphurization is effected. Experiments
conducted by Mr. Bradford, the chief assayer, demonstrated that, at a
temperature of 400 deg. C., the sulphide slime is converted into basic
sulphate, while at a temperature of 800 deg. C. the material becomes
sintered owing to the decomposition of the basic sulphate and the
formation of fusible silicate of lead.
In practice, the sulphur contents of the material, which originally
are about 14 per cent., become reduced to from 6.5 to 8.5 per cent.,
half in the form of basic sulphate and half as sulphides; much of the
material sinters and becomes matted together in a fairly solid mass.
The heaps are built without chimneys of any kind; a strip about 5
ft. wide along the crest of the pile is left uncovered by plastered
slime, and this, together with the open way in which the lumps are
built in, allows a natural draft to be set up, which can be regulated
by partly closing the open ends of the flues at the base of the pile.
Masonry kilns were used in the earlier stages with good results, which,
however, were not so much better than those obtained by the heap method
as to justify the expense of building, taking into consideration, too,
the extra cost of handling the roasted material in the necessarily more
confined space.
Much interest has been taken in the chemical reactions which take
place in the operation of desulphurization of these slimes, it being
contended, on the one hand, that the unexpectedly rapid roast which
takes place may be due to the sulphide being in a very fine state of
subdivision, and more or less porous, thus allowing the air ready
access to the sulphur, producing sulphurous acid gas (SO₂). On the
other hand, others, of whom Mr. Carmichael is the chief exponent, claim
that several reactions take place during the operation, connected
with the rhodonite and lime compounds present in the slimes, which he
describes as follows:
“The temperature of the kilns having reached a dull red heat, the
rhodonite (silicate of manganese) is converted into manganous oxide
and silica; at a rather higher temperature the calcium compounds are
also split up, with formation of calcium sulphide, the sulphur being
provided by the slimes. The air permeating the mass oxidizes the
manganese oxide and calcium sulphide into manganese tetroxide and
calcium sulphate respectively, as shown as follows;
3MnO + O = Mn₃O₄
CaS + 4O = CaSO₄,
and, as such, are carriers of a form of concentrated oxygen to the
sulphide slimes, with a corresponding reduction to manganous oxide and
calcium sulphide, as shown by the following equation, in the case of
lead:
PbS + 4Mn₃O₄ = PbSO₄ + 12MnO
PbS + CaSO₄ = PbSO₄ + CaS.
The oxidation of the manganous oxide and calcium sulphide is repeated,
and these alternate reactions recur until the desulphurization ceases,
or the kiln cools down to a temperature below which oxidation cannot
occur. These reactions, being heat-producing, provide part of the heat
necessary for desulphurization, which is brought about by certain
concurrent reactions between metallic sulphates and sulphide.
“The first that probably occurs is that in which two equivalents of the
metallic sulphide react on one of the metallic sulphate with reduction
to the metal, metallic sulphide, and sulphurous acid, as shown by the
following equation in the case of lead:
2PbS + PbSO₄ = 2Pb + PbS + 2SO₂.
“The metal so formed, in the presence of air, is oxidized, and in this
state reacts on a further portion of the metallic sulphide produced,
with an increased formation of metal and evolution of sulphurous acid,
according to the following equation, in the case of lead:
2PbO + PbS = Pb + SO₂.
“The metal so produced in this reaction is wholly reoxidized by the
oxygen of the air current, and being free to react on still further
portions of the metallic sulphide, repeats the reaction, and becomes
an important factor in the desulphurizing of the undecomposed portion
of the material. As the desulphurization proceeds, and the sulphate of
metal accumulates, reactions are set up between the metallic sulphide
and different multiple proportions of the metallic sulphate, with the
formation of metal, metallic oxide, and evolution of sulphurous acid,
as follows:
“With two equivalents of metallic sulphate to one equivalent of
metallic sulphide, in the case of lead, according to the following
equation:
PbS + 2PbSO₄ = 2PbO + Pb + 3SO₂.
“With three equivalents of metallic sulphate to one of metallic
sulphide, in the case of lead, according to the following equation:
PbS + 3PbSO₄ = 4PbO + 4SO₂.”
The volatility of sulphide of lead—especially in the presence of an
inert gas such as sulphurous acid—being greater than that of the
sulphate, oxide, or the metal itself, it might be thought that the
conditions are conducive to a serious loss of lead. This, however, is
reduced to a minimum, owing to the easily volatilized sulphide being
trapped, as non-volatile sulphate, by small portions of sulphuric
anhydride (SO₃), which is formed by a catalytic reaction set up
between the hot ore, sulphurous acid, and the air passing through
the mass. Owing to the non-volatility of the silver compounds in the
slimes, the loss of this metal has been found to be inappreciable. The
zinc contents of the slime are reduced appreciably, thus rendering the
material more suitable for smelting. After desulphurization ceases,
a few days are allowed for cooling off. On the breaking up of the
mass for despatch to the smelters, as much of the lower portion of
the walls is left intact as possible, so that it can be utilized for
the next roast, thus avoiding the re-building of the whole of the
walls.[10]
THE PREPARATION OF FINE MATERIAL FOR SMELTING
BY T. J. GREENWAY
(January 12, 1905)
In the course of smelting, at the works of the company known as the
Broken Hill Proprietary Block 14, material which consisted chiefly of
silver-lead concentrate and slime, resulting from the concentration
of the Broken Hill complex sulphide ore, I had to contend with all
the troubles which attend the treatment of large quantities of finely
divided material in blast furnaces. With the view of avoiding these
troubles, I experimented with various briquetting processes; and,
after a number of more or less unsatisfactory experiences, I adopted a
procedure similar to that followed in manufacturing ordinary bricks by
what is known as the semi-dry brick-pressing process. This method of
briquetting not only converts the finely divided material cheaply and
effectively into hard semi-fused lumps, which are especially suitable
for the heavy furnace burdens required by modern smelting practice, but
also eliminates sulphur, arsenic, etc., to a great extent; therefore,
it is capable of wide application in dealing with concentrate, slime,
and other finely divided material containing lead, copper and the
precious metals.
This briquetting process comprises the following series of operations:
1. Mixing the finely divided material with water and newly slaked lime.
2. Pressing the mixture into blocks of the size and shape of ordinary
bricks.
3. Stacking the briquettes in suitably covered kilns.
4. Burning the briquettes, so as to harden them, without melting, at
the same time eliminating sulphur, arsenic, etc.
1. The material is dumped into a mixing plant, together with such
proportions of screened slaked lime (usually from three to five per
cent.) and water as shall produce a powdery mixture which will, on
being squeezed in the hand, cohere into dry lumps. In preparing the
mixture, it is well to mix sandy material with suitable proportions
of fine, such as slime, in order that the finer material may act as a
binding agent.
The mixer used by me consists of an iron trough, about 8 ft. long,
traversed by a pair of revolving shafts, carrying a series of knives
arranged screw-fashion; and so placed that the knives on one shaft
travel through the spaces between the knives on the other shaft.
The various materials are dumped into one end of the mixing trough,
from barrows or trucks, and are delivered continuously at the other
end of the trough, into an elevator which conveys the mixture to the
brick-pressing plant.
2. The plant employed was the semi-dry brick-press. This machine
receives the mixture from the elevators, and delivers it in the form
of briquettes, which can at once be stacked in the kilns. It was found
that such material as concentrate and slime has comparatively little
mobility in the dies during the pressing operation; this necessitates
the use of a device which provides for the accurate filling of the
dies. It was also found that the materials treated by smelters vary
in compressibility, and this renders necessary the adoption of a
brick-pressing plant having plungers which are forced into the dies by
means of adjustable springs, brick-presses having plungers actuated by
rigid mechanism being extremely liable to jam and break.
3. Briquettes made from such material as concentrate and slime vary
in fusibility; they are also combustible, and while being burned they
produce large quantities of smoke containing sulphurous acid and other
objectionable fumes. It is therefore necessary that such briquettes be
burned in kilns provided with arrangements for accurately controlling
the burning operations, and for conveniently disposing of the smoke.
Suitable kilns, which will contain from 30 to 50 tons of briquettes
per setting, are employed for this purpose. Regenerative kilns of the
Hoffman type might be used for dealing with some classes of material,
but, for general purposes, the kilns as designed here will be found
more convenient.
The briquettes are stacked according to the character of the material
and the object to be obtained. The various methods of stacking, and the
reasons for adopting them, can be readily learned by studying ordinary
brick-burning operations in any large brick-yard. After the stacking
is complete the kiln-fronts are built up with burnt briquettes produced
in conducting previous operations, and all the joints are well luted.
4. In burning briquettes made from pyrite or other self-burning
material, it is simply necessary to maintain a fire in the kiln
fireplaces for a period of from 10 to 20 hours. When it is judged that
this firing has been continued long enough, the fire-bars are drawn
and the fronts are luted with burnt briquettes in the same manner as
the kiln-fronts. Holes about two inches square are then made in these
lutings, through which the air required for the further burning of the
briquettes is allowed to enter the kilns under proper control. After
the fireplaces are thus closed the progress of the burning, which
continues for periods of from three to six days, is watched through
small inspection holes made in the kiln-fronts; and when it is seen
that the burning is complete the fronts are partially torn away,
in order to accelerate the cooling of the burnt briquettes, which
are broken down and conveyed to the smelters as soon as they can be
conveniently handled.
When briquettes made from pyrite concentrate, or of other free-burning
material, are thus treated, they are not only sintered but they are
also more or less effectively roasted, and it may be taken for granted
that any ore which can be effectively roasted in the lump form in kilns
or stalls will form briquettes that will both sinter and roast well;
indeed, one may say more than this, for briquettes which will sinter
and roast well can be made from many classes of ore that cannot be
effectively treated by ordinary kiln-and stall-roasting operations;
and, moreover, good-burning briquettes may be made from mixtures of
free-burning and poor-burning material. Briquettes containing large
proportions of pyrite or other free-burning material will, unless the
air-supply is properly controlled, often heat up to such an extent as
to fuse into solid masses, much in the same manner as matte of pyritic
ore will melt when it is unskilfully handled in roasting. In dealing
with material which will not burn freely, such as roasted concentrate,
the briquetting is conducted with the intention of sintering the
material; and in this case the firing of the kilns is continued for
periods of from three to four days, the procedure being similar in
every way to that followed in burning ordinary bricks.
When conducting my earlier briquetting operations I made the
briquettes by simply pugging the finely divided material, following
a practice similar to that adopted in producing “slop-made” bricks
by hand. This method of making the briquettes was attended with a
number of obvious disadvantages, and was abandoned as soon as the
semi-dry brick-pressing plant became available. The extent to which
this process, or modifications of it, may be applied is shown by the
fact that, following upon information given by me, the Broken Hill
Proprietary Company adopted a similar method of sintering and roasting
slime, consisting of about 20 per cent. galena, 20 per cent. blende,
and 60 per cent. silicious gangue. The procedure followed in this
case consisted of simply pugging the slime, and running the pug upon
a floor to dry; afterward cutting the dried material into lumps by
means of suitable cutting tools, and then piling the lumps over firing
foundations, following a practice similar to that pursued in conducting
ordinary heap-roasting. This company is now treating from 500 to 1000
tons of slime weekly in this manner. It is, however, certain that
better results would attend the treatment of this material by making
this slime into briquettes and burning them in kilns.
The cost of briquetting and burning material in the manner first
described, with labor at 25c. per hour, and wood or coal at $4 per ton,
amounts to from $1 to $1.50 per ton of material.
THE BRIQUETTING OF MINERALS
BY ROBERT SCHORR
(November 22, 1902)
The value of briquetting in connection with metallurgical processes and
the manufacture of artificial stone is well understood and appreciated.
In smelting plants there is always more or less flue dust, fine ores,
and sometimes fine concentrates to be treated, but the charging
of such fine material directly into a furnace would cause trouble
and irregularities, and would lessen its capacity also. As mineral
briquetting cannot be effected without considerable wear upon the
machinery and without quite appreciable expense in binder, labor, and
handling, many smelters try to avoid it.
The financial question, however, is not as serious as it may at first
appear, and taking the large output of modern briquetting machines in
consideration, the cost for repairs amounts only to a few cents per ton
of briquetted material. The total cost depends in the first place on
the cost of labor, power and the binder, and in most American smelters
it varies between $0.65 and $1.25 per ton of briquettes.
Ordinary brick presses, with clay as a binder, were used in Europe as
well as in this country, but they are too slow and expensive for large
propositions and the presence of clay is usually undesirable.
The English Yeadon (fuel) press has also been used for some years at
the Carlton Iron Company’s Works at Ferryhill in England, and at the
Ore and Fuel Company’s plant at Coatbridge in the same country; also by
some Continental firms. Dupuis & Sons, Paris, furnished a few presses
which are mostly used for manganese and iron ores and pyrites. In
some localities coke dust is added. The making of clay briquettes or
mud-cakes is the crudest form of briquetting; but while heat has to
be expended to evaporate the 40 to 50 per cent. of moisture in them,
and while considerable flue dust is made, this method is better than
feeding fine ore or flue dust directly into the furnace.
The only other method of avoiding briquetting is by fusing ore fines in
slagging reverberatory furnaces and by adding flue dust in the slagging
pit, thus incorporating it with the slagging ore. This is practised
sometimes in silver-lead smelters, but in connection with copper or
iron smelters it is not practicable.
In briquetting minerals a thorough mixing and kneading is of the first
importance. If this is done properly a comparatively low pressure will
suffice to create a good and solid briquette, which after six to eight
hours of air-drying, or after a speedier elimination of the surplus of
moisture in hot-air chambers, will be ready for the furnace charge. A
good briquette should permit transportation without excessive breakage
or dust a few hours after being made, and it should retain its shape in
the furnace until completely fused, so as to create as little flue dust
as possible. The briquette should be dense, otherwise it will crumble
under the influence of bad weather.
The two presses on the American machinery market are the type built by
the Chisholm, Boyd & White Company, of Chicago, and the briquetting
machine manufactured by the H. S. Mould Company, of Pittsburg. Both are
extensively used, and in many metallurgical plants it will pay well to
adopt them.
From 4 to 6 per cent. of milk of lime is generally used as binder,
and this has a desirable fluxing influence also. A complete outfit
comprises, besides the press, a mixer for slacking the lime, and a
feed-pump which discharges the liquid in proportion into the main mixer
wherein the ore fines, flue dust, or concentrates are shoveled.
The Chisholm, Boyd & White Company’s press makes 80 briquettes per
minute, which, with a new disk, are of 4 in. diameter and 2½ in. hight,
thus giving about 872 cu. ft. of briquette volume per 10 hours, or 50
to 80 tons, depending on the weight of the material. With the wear of
the disk the hight of the briquettes is reduced and consequently the
capacity of the machine also. The disk weighs about 1600 lb., and as
most large smelters have their own foundries it can be replaced with
little expense. About 30 effective horse-power is usually provided for
driving the apparatus. The machine is too well known to metallurgists
and engineers to require further comment or description.
The H. S. Mould Company has also succeeded in making its machine a
thorough practical success. This machine is a plunger-type press. The
largest press built employs six plungers, and at 25 revolutions it
makes 150 briquettes of 3 in. diameter and 3 in. hight, or 1080 cu. ft.
per 10 hours. Its rated capacity is 100 tons per 10 hours.
In using a plunger-type press the material should not contain more
than 7 per cent. mechanical moisture. If wet concentrates have to
be briquetted it is necessary to add dry ore fines or flue dust to
arrive at a proper consistency. The briquettes are very solid and only
air-drying for a few hours is necessary.
The cylindrical shape of briquettes is very good, as it insures
a proper air circulation in the furnace and consequently a rapid
oxidation and fusion.
The wear of the Mould Company’s press is mostly confined to the chilled
iron bushings and to the pistons. Auxiliary machinery consists of
the slacker, the feeder and the main mixer. The press is of a very
substantial design, and it is claimed that the cost of repairs does not
amount to more than 3c. per ton of briquettes.
Wear and tear is unavoidable in a crude operation like briquetting; to
treat flue dust, ore fines, and fine concentrates successfully, it is
almost absolutely necessary to resort to it.
Edison used a number of intermittent-acting presses at his magnetic
iron-separation works in New Jersey, but this plant shut down some time
ago.
A BRICKING PLANT FOR FLUE DUST AND FINE ORES
BY JAMES C. BENNETT
(September 15, 1904)
The plant, which is here described, for bricking fine ores and flue
dust, was designed and the plans produced in the engineering department
of the Selby smelter. The machinery contained in the plant consists of
a Boyd four-mold brick press, a 7 ft. wet pan or Chile mill, a 50 h.p.
induction motor, and a conveyor-elevator, together with the necessary
pulleys and shafting.
The press, Chile mill, and motor need no special mention, as they all
are from standard patterns and bought, without alterations, from the
respective builders. The Chile mill was purchased from the builders
of the brick press. The conveyor-elevator was built on the premises
and consists of a 14 in. eight-ply rubber belt, with buckets of sheet
steel placed at intervals of 6 in., running over flanged pulleys. The
buckets, or more properly speaking the flights, are made from No.
12 steel plate, flanged to produce the back and ends, with the ends
secured to the flanged bottom by one rivet in each. The plant has been
in operation for sixteen months and there have been few or no repairs
to the elevator, except to renew the belt, which is attacked by the
acid contained in the charges. This first belt was in continuous use
for nine months. As originally designed, the capacity was 100 tons per
day of 12 hours, but this was found to require a speed so high that
the workmen were unable to handle the output of the press. The speed
was, consequently, reduced about 25 per cent., which brings the output
down to about 75 tons per day. This output, as expressed in weight,
naturally varies somewhat owing to the variation in the weight of the
material handled.
It is probable that the capacity could be increased to about 90 tons
by enlarging the bricks, which could be done, but would require a
considerable amount of alteration in the machine, as it is designed to
produce a standard sized building brick. By this method of increase,
however, the work of handling would not be materially increased,
because the number of bricks would be the same as with the present
output of 75 tons; there would be about 16 per cent. more to handle,
by weight. Working on the basis of 100 tons capacity, the bins were
designed to afford storage room for about three days’ run, or a little
over 300 tons. The bins are made entirely of steel, in order that
the hot material may be dumped into them directly from the roasting
furnaces, thus saving one handling. In order that there may be room
for several kinds of material, the bins are divided into seven
compartments, three on one side and four on the other. The lower part
is of ⅜ in. steel plate, and the upper, about one-half the hight, of
5/16 in. plate.
It may be well to call attention to the method of handling the
material, preparatory to its delivery to the brick press. The bins are
constructed, as will be seen by the drawing, with their floor set 2.5
ft. above the working floor, which enables the workmen to reach the
material with a minimum effort. The floor of the bins project 2.5 ft.
in front of the face, thus forming a platform on which the shoveling
may be done without the necessity of bending over. In this projecting
platform are cut rectangular holes 12 × 18 in., which are placed
midway between the openings in the front of the bins and furnished
with screens to stop any stray bolts or other coarse material that
might injure the press. This position of the holes through the platform
was adopted so that, in the event of the material running out beyond
the opening in the face, it would not fall directly upon the floor.
Two buckets are provided, with a capacity of 7 cu. ft. each, which is
the size of a single charge of the Chile mill. These buckets have a
hopper-shaped bottom fixed with a swinging gate which is operated by
the foot; thus the bucket can be run over the pan of the Chile mill and
the charge dumped directly into it. The buckets run on an overhead iron
track (1 in. by 3 in.) hung 7 ft. in the clear, above the floor.
The method of making up the charge is as follows: The bucket is
run under the hole in the platform nearest to the compartment
containing the material of which the charge is partly composed, and
a predetermined number of shovelfuls is drawn out and put into the
bucket, which is then pushed on to the next compartment from which
material is wanted, where the operation is repeated. After charging
into the bucket the requisite amount of ore or flue dust, the bucket
is run to the back of the building, where the necessary amount of lime
(slaked) is added. By putting the lime in last, it is so surrounded by
the dust or ore that it has not the opportunity to stick to the sides
of the bucket in discharging, as it otherwise would.
[Illustration: FIG. 1 (_a_).—Plant for Bricking Ores, Selby Smelter.
(Plan.)]
The number of men required to operate the entire plant, exclusive
of those employed in bringing the material to the bins and emptying
the cars into them, is 12, placed as follows; One preparing the lime
for use, one removing the charge from the mill and supplying the
elevator-conveyor, which is accomplished by means of a specially
shaped, long-handled shovel; one keeping the supply spout of the press
clear (an attempt was made to do this mechanically, but was found to be
unsuccessful, owing to the extremely sticky nature of the material, and
so was discarded in favor of manual labor); one to control the press in
case of mishap and to keep the dies clean; one oiler; three receiving
the bricks from the press and taking the brick-loaded cars from the
press to the drying-house, and two placing the bricks on the shelves.
[Illustration: FIG. 1 (_b_).—Plant for Bricking Ores, Selby Smelter.
(Elevation.)]
The drying-house scarcely requires description; it is but a roofed
shed, without sides, fitted with stalls into which the bricks are set
on portable shelves, as close as working conditions will permit. The
means of drying, at the present time, is by the natural circulation
of air, but a mechanical system is in contemplation, by which the
air will be drawn into the building from the outside and forced to
find its way out through the bricks. The drying-house is adjacent to
the pressing plant, in fact forms the back of it, so that there is a
minimum distance to haul the product. The time required for drying the
bricks sufficiently for them to withstand the necessary handling is,
depending on the weather, from two to eight days, the usual time being
about three days.
PART IV
SMELTING IN THE BLAST FURNACE
MODERN SILVER-LEAD SMELTING[11]
BY ARTHUR S. DWIGHT
(January 10, 1903)
The rectangular silver-lead blast furnace developed in the Rocky
Mountains has an area of 42 × 120 to 48 × 160 in. at the tuyeres; 54
× 132 to 84 × 200 in. at the top; and hight from tuyere level to top
of charge of 15 to 21 ft. Such a furnace smelts 80 to 200 tons of
charge (ore and flux, but not slag and coke) per 24 hours. The slag
that has to be resmelted amounts to 20 to 60 per cent. of the charge.
Coke consumption is 12 to 16 per cent. of the charge. The blast
pressure ranges from 1.5 to 4 lb. per square inch, averaging close to
2 lb. Gases of hand-charged furnaces are taken off through an opening
below the charge-floor, the furnace being fed through a slot (about
20 in. wide, extending nearly the whole length of the furnace) in the
iron floor-plates; or through a hood (brick or sheet iron) above the
charge-floor level, with a down-take to the flues, charge-doors being
provided on each side of the hood, extending preferably the whole
length of the furnace and usually having a sill a few inches high which
compels the feeder to lift his shovel.
When a silver-lead blast furnace is operating satisfactorily, the
following conditions should obtain; (1) A large proportion of the lead
in the charge should appear as direct bullion-product at the lead-well.
(2) The slag should be fluid and clean. (3) The matte should be low
in lead. (4) The furnace should be cool and quiet on top, making a
minimum quantity of lead-fume and flue-dust, and the charges should
descend uniformly over the whole area of the shaft. (5) The furnace
speed should be good. (6) The furnace should be free from serious
accretions and crusts; that is to say, the tuyeres should be reasonably
bright and open, and the level of the lead in the lead-well should
respond promptly to variations of pressure, caused by the blast and by
the hight of the column of molten slag and matte inside the furnace—an
indication that ample connection exists between the smelting column and
the crucible. Good reduction (using that term to express the degree in
which the furnace is manifesting its reducing action) is obtained when
the first three of the above conditions are satisfied.
For any given furnace there are five prime factors, the resultant of
which determines the reduction, namely: (_a_) Chemical composition
of the furnace charges; (_b_) proportion and character of fuel;
(_c_) air-volume and pressure, to which might perhaps also be added
temperature of blast; for, although hot blast has not yet been
successfully applied in lead-smelting practice, I believe it is only
a question of time when it will be; (_d_) dimensions and proportions
of smelting furnace; (_e_) mechanical character and arrangement of the
smelting column.
All but one of the above factors can be intelligently gaged. The
mechanical factor, however, can be expressed only in generalities and
indefinite terms. A wise selection of ores and proper preliminary
preparation, crushing the coarse and briquetting the fine, will do
much to regulate it, but all this care may be largely nullified by
careless feeding. The importance and possibilities of the mechanical
factor are generally overlooked and its symptoms are wrongly diagnosed.
For instance, the importance of slag-types has undoubtedly been
considerably exaggerated at the expense of the mechanical factor.
Slags seldom come down exactly as figured. We must know our ores and
apply certain empirical corrections to the iron, sulphur, etc., based
on previous experience with the ores; but these empirical corrections
may represent also an unformulated expression of the influence of the
mechanical factor on the reduction—a function, therefore, of the ruling
physical complexion of the ores, and the peculiarities of the feeding
habitually maintained in the works concerned. With a given ore-charge
large reciprocal variations may be produced in the composition of
slag and matte by merely changing the mechanical conditions of the
smelting column, and since the efficient utilization of both fuel and
blast must be controlled in the same way, the mechanical factor may be
considered, perhaps, the dominating agent of reduction. Inasmuch as
there is no way of gaging it, however, the only recourse is to seek a
correct adjustment and maintain it as a positive constant, after which
slag, fuel and blast may be with much greater certainty adjusted toward
efficiency of furnace work and metal-saving.
_Behavior of Iron._—The output of lead is so dependent upon the
reactions of the iron in the charge that the chief attention may well
be fixed upon that metal as the key to the situation. The success of
the process depends largely upon reducing just the right amount of
iron to throw the lead out of the matte, the remainder of the iron
being reduced only to ferrous oxide and entering the slag. Too much
iron reduced will form a sow in the hearth. Iron is reduced from its
oxides principally by contact with solid incandescent carbon, and by
the action of hot carbon monoxide. Reduction by solid carbon is the
more wasteful, but there is in lead smelting an even more serious
objection to permitting the reduction to be accomplished by that means,
which leads to comparatively hot top and more or less volatilization of
lead. Reduction by carbon monoxide is the ideal condition for the lead
furnace. It means keeping the zone of incandescence low in the charge
column, leaving plenty of room above for the gases to yield up their
heat to, and exercise their reducing power on, the descending charge,
so that by the time they escape they will be well-nigh spent. Their
volume and temperature will be diminished, and the low velocity of
their exit will tend to minimize the loss of lead in fume and flue dust.
The idea that high temperatures in lead blast furnaces should be
avoided is based on a misconception. Temperatures must exist which
are sufficiently high to volatilize all the lead in the charge, if
other conditions permit. A high temperature before the tuyeres means
fast smelting; and fast smelting, under proper conditions, means a
shortening of the time during which the lead is subject to scorifying
and volatilizing influences. A rapidly descending charge, constantly
replenished with cold ore from above, absorbs effectively the heat of
the gases and acts as a most efficient dust and fume collector. In
considering long flues, bag-houses, etc., it should be kept in mind
that the most effective dust collector ought to be the furnace itself.
In the practice of twelve years ago and earlier, particularly when
using mixed coke and charcoal, reduction by carbon was probably the
rule; and the percentage of fuel required was very high. There is good
reason to think we have still much room for improvement along this line
in our average practice of today.
_Volume of Blast._—It is customary to supply a battery of furnaces
from a large blast main, connected with a number of blowers. Inasmuch
as the air will take preferably the line of least resistance, if the
internal resistance of any one furnace be increased the volume of air
it will take will be diminished and the others will be favored unduly.
Only by keeping all the furnaces on approximately the same charge, with
the same hight of smelting column, can anything like uniformity of
operation and close regulation be secured. The rational plan would seem
to be to have a separate blower, of variable speed, directly connected
to each furnace, but this plan, which has had a number of trials, has
usually been abandoned in favor of the common blast main. Trials by
myself, extending over considerable periods, have been so uniformly
favorable, however, that I am forced to ascribe the failure of others
to some outside reason.
The peculiar atmosphere required in the lead blast furnace depends
upon the correct proportion of two counteractive elements, carbon and
oxygen. If given too much air the furnace will show signs of deficient
reduction, commonly interpreted as calling for more fuel, which will
be sheer waste since its object is to burn up surplus air. There will
be an additional waste through the extra coal burned under the steam
boilers. The true remedy would be to cut down the quantity of air.
Burning up excessive coke is as hard work as smelting ore. Too much
fuel invariably slows up a furnace; it also drives the fire upward and
gives predominance to reduction by solid carbon. The maintenance of a
minimum fuel percentage, with a correctly adjusted volume of air, will
tend to promote the conditions under which iron will be reduced by the
gases, rather than by solid carbon.
_Pressure of Blast._—Pressure necessarily involves resistance; and
the blast-pressure, as registered by a simple mercury-gage on the
bustle-pipe, may be increased in two ways: (1) By increasing the volume
of air forced through the interstices in the charge. This is the
wrong way; but, unfortunately, it is only too common in our practice,
and therefore deserves to be mentioned, if only to be condemned. (2)
By leaving the volume of air unchanged, but increasing the friction
offered by the interstitial channels, either by making them smaller in
aggregate cross-section (which means a finer charge), or by making them
longer (which means a higher smelting column). A correctly graduated
internal resistance is, therefore, the only true basis for a high blast
furnace, which, when so produced, will bring about rapid smelting, a
low zone of incandescence, and a very vigorous action upon the ores by
the gases in their retarded ascent through the charge column. These
conditions promote the reduction of iron by CO. The adjustment of
internal resistance, which is thus clearly the main factor, can be
accomplished only by the correct feeding of the furnace.
_Feeding the Charge._—It is self-evident that, the more thorough the
preliminary preparation of the charge before it reaches the zone of
fusion, the more rapidly can the actual smelting proceed. A piece of
raw ore that finds itself prematurely at the tuyeres, without having
been subjected to the usual preparatory processes of drying, heating,
reduction, etc., must remain there until it is gradually dissolved or
carried away mechanically in the slag. Any such occurrence must greatly
retard the process. It would seem, by the same reasoning, that an
intimate mixture of the ingredients of the charge should expedite the
smelting, and I advocate the intimate mixture of the charge ingredients
in all cases.
The theory of feeding is simple, but not so the practice. If the
charge column were composed of pieces of uniform size, the ascending
gases would find the channel of least resistance close to the furnace
walls and would take it preferably to the center of the shaft. The
more restricted channel would necessitate a higher velocity, so that
not only would the center of the charge be deprived of the action of
the gases, but also the portion traversed would be overheated; many
particles of ore would be sintered to the walls or carried off as flue
dust; slag would form prematurely; fuel would be wasted; in short,
all the irregularities and losses which accompany over-fire would be
experienced. In practice the charge is never uniform, but is a mixture
of coarse and fine. By lodging the finer material close to the walls
and placing the coarser in the center, an adjustment may be made which
will cause the gases to ascend uniformly through the smelting column.
A furnace top smoking quietly and uniformly over its whole area is the
visible sign of a properly fed furnace.
_Effect of Large Charges._—It has frequently been remarked that,
within certain limits, large charges give more favorable results
than small ones; and numerous attempts have been made to account
for this fact. My observations lead me to offer the following as a
rational explanation—at least in cases where ore and fuel are charged
in alternate layers. Large ore-charges mean correspondingly large
fuel-charges. The gases can pass readily through the coke; and hence
each fuel-zone tends to equalize the gas currents by giving them
another opportunity to distribute themselves over the whole furnace
area, while each layer of ore subsequently encountered will blanket the
gases, and compel them to force a passage under pressure, which is the
manner most favorable to effective chemical action.
In mechanically fed furnaces the charges of ore and fuel are usually
dropped in simultaneously from a car and the separate layers thus
obliterated, and the distributing zones which are such a safeguard
against the consequences of bad feeding are lacking, hence more care
must be exercised to secure proper placing of the coarse and fine
material. This may throw some light on the failure of most of the early
attempts at mechanical feeding.
_Mechanical Character of Charge._—Very fine charges blanket the gases
excessively and cause them to break through at a few points, forming
blow-holes, which seriously disturb the operation, cause loss of raw
ore in the slag, and are accompanied by all the evils of over-fire. A
charge containing a few massive pieces, the rest being fine, is a still
more unfavorable combination. A very coarse charge permits too ready an
exit to the gases, and in the end tends likewise to over-fire and poor
reduction. The remedy is to briquette the fine ore (though preferably
not all of it), and crush the coarse to such degree as to approach an
ideal result, which may be roughly described as a mixture in which
about one-third is composed of pieces of 5 to 2 in. in diameter,
one-third pieces of 2 to 0.5 in., and the remaining third from 0.5 in.
down. The coke is better for being somewhat broken up before charging,
and a reasonable amount of coke fines, such as usually accompanies
a good quality of coke, is not in the least detrimental. The common
practice of handling the coke by forks and throwing away the fines
is to be condemned as an unwarranted waste of good fuel. The slag on
the charge should be broken to pieces at most 6 in. in diameter. The
common practice of throwing in whole butts of slag-shells is bad.
There is no economy in using the slag hot; cold charges, not hot,
are what we want. A reasonable amount of moisture in the charge is
beneficial, providing it be in such form as to be readily dried out. It
is often advantageous to wet the ore mixtures while bedding them, or
to sprinkle the charges before feeding. The driving off of this water
must consume fuel, but not so much as if the smelting zone crept up.
Large doses of water applied directly to the furnace are unpardonable
under any circumstances, however, though they are sometimes indulged
in as a drastic measure to subdue excessive over-fire when other and
surer means are not recognized. One of the chief merits of moderate
sprinkling before charging is that it gives in many cases a more
favorable mechanical character, approximating a lumpy condition in too
fine a charge, and assisting to pack a too coarse one.
_Different Behavior of Coarse and Fine Ore._—In taking up a shovelful
of ore, the fine will be observed to predominate in the bottom and
center, and the coarse on the top and sides. When thrown from the
shovel, the coarse will outstrip the fine and fall beyond it. In making
a conical pile the coarse ore will roll to the base, leaving the fine
near the apex. This difference in the action of the mobile coarse ore
and the sluggish fines is the key to the practical side of feeding,
both manual and mechanical. It is not sufficient to tell the feeder to
throw the coarse in the middle and the fine against the sides; if it be
easier to do it some other way such instructions will count for little.
The desired result can be best secured by making the right way easier
than the wrong way.
It is generally conceded that the open-top furnaces, fed by hand
through a slot in the floor-plates, do not give as satisfactory results
as the hooded furnaces with long feed-doors on both sides. In the
open-top furnace it is comparatively difficult to throw to the sides;
the narrower the slot the greater the difficulty. The major part of the
charge will drop near the center, making that place higher than the
sides. The fine ore will tend to stay where it falls, while the coarse
will tend to roll to the sides, thus leading to an arrangement of the
charge just the reverse of what it ought to be. In the hooded furnace
most of the material will naturally fall near the doors, causing the
sides to be higher than the center toward which the coarse will roll,
while the force of the throw as the ore is shoveled in will also have
a tendency to concentrate the coarse material in the center.
Once a proper balance of conditions has been found, absolute
regularity of routine is the secret of good results. An experienced
and intelligent feeder owes his merit to his conscientious regularity
of work. He may have to vary his program somewhat when he encounters
a furnace that is suffering from the results of bad feeding by a
predecessor; but his guiding principle is first to restore regularity,
and then maintain it. A poor feeder can bring about, in a single
shift, disorders that will require many days to correct, if indeed
they are corrected at all during the campaign. The personal element is
productive of more harm than good.
_Mechanical Feeding._—If it be admitted that the work of a feeder
is the better the more it approximates the regularity of that of a
machine, it ought to be desirable to eliminate the personal factor
entirely and design a machine for the purpose, which would be a
comparatively simple matter if it be known just what we want to
accomplish. No valid ground now exists for prejudice against mechanical
feeding in lead smelting. It is in successful operation in a number
of large works, and is being installed in others. Our furnaces have
outgrown the shovel; we have passed the limit of efficiency of the
old methods of handling material for them. We must come to mechanical
feeding in spite of ourselves. But whatever may be the motive leading
to its introduction, its chief justification will be discovered,
after it has been successfully installed and correctly adjusted, in
the consequent great improvement of general operating results, metal
saving, etc. It will remove one of the most uncertain factors with
which the metallurgist has to deal, thereby bringing into clearer view
for study and regulation the other factors (fuel and blast proportion,
slag composition, etc.) in a way that has hardly been possible under
the irregularities consequent upon hand feeding.
MECHANICAL FEEDING OF SILVER-LEAD BLAST FURNACES[12]
BY ARTHUR S. DWIGHT
(January 17, 1903)
_Historical._—A silver-lead furnace fed by means of cup and cone was in
operation in 1888 at the works of the St. Louis Smelting and Refining
Company at St. Louis, Mo., but it is probable that previous attempts
had been made, since Hahn refers (“Mineral Resources of the United
States,” 1883) in a general way to experiments with this device, which
were unsuccessful because the heat crept up in the furnace and gave
over-fire. At the time of my visit to the St. Louis works (in 1888)
the furnaces were showing signs of over-fire, but this may not have
been their characteristic condition. A. F. Schneider, who built the St.
Louis furnaces, afterward erected, at the Guggenheim works at Perth
Amboy, N. J. , round furnaces with cup and cone feeders, but although
good results are said to have been obtained, the running of refinery
products is no criterion of what they would do on general ore smelting.
_Cup and Cone Feeders._—The cup and cone is an entirely rational device
for feeding a round furnace, but is quite unsuitable for feeding a
rectangular one. Furnaces of the latter type were installed for copper
smelting at Aguas Calientes, Mex., with two sets of circular cup and
cone feeders, but disastrous results followed the application of this
device to lead furnaces. The reason is clear when it is considered that
a circular distribution cannot possibly conform to the requirements
of a rectangular furnace. A more rational device was designed for the
works at Perth Amboy, N. J.
[Illustration: FIG. 2.—Perth Amboy, N. J. , Lead Furnace. Vertical
section at right angles to Fig. 3.]
_Pfort Curtain._—About ten years ago some of the American smelters
adopted the Pfort curtain, which, as adapted to their requirements,
consisted of a thimble of sheet iron hung from the iron deck plates so
as to leave about 15 in. of space between it and the furnace walls,
this space being connected with the down-take of the furnace. The
thimble was kept full of ore up to the charge-floor. This device was
popular for a time, chiefly because it prevented the furnace from
smoking and diminished the labor of feeding, but it was found to give
bad results in the furnaces, it being impossible to observe how the
charge sunk (except by dropping it below the thimble), while the
curtain had to be removed in order to bar down accretions, and, most
important, it caused irregular furnace work and high metal losses,
because it effected a distribution of the coarse and fine material
which was the reverse of correct, the evil being emphasized by the
taking off of the gases close to the furnace walls.
[Illustration: FIG. 3.—Perth Amboy, N.J., Lead Furnace. Vertical
section at right angles to Fig. 2.]
_Terhune Gratings._—R. H. Terhune designed a device (United States
patent No. 585,297, June 29, 1897), which comprised two grizzlies,
one on each side of the furnace, sloping downward from the edge of
the charge-floor toward the center line of the furnace. The bars
tapered toward the center of the furnace, the open spaces tapering
correspondingly toward the sides, so that as the charge was dumped on
them a classification of coarse and fine would be effected. This device
is correct in conception.
_Pueblo System._—In the remodeling of the plant of the Pueblo Smelting
and Refining Company in 1895, under the direction of W. W. Allen,
mechanical feeding was introduced, and the system was the first one to
be applied successfully on a large scale. The furnaces of this plant
are 60 × 120 in. at the tuyeres, with six tuyeres, 4 in. in diameter
on each side, the nozzles (water cooled) projecting 6 in. inside the
jackets. The hight of the smelting column above the tuyeres is 20 ft.
The gases are taken off below the charge-floor, and the furnace tops
are closed by hinged and counter-weighted doors of heavy sheet iron,
opened by the attendant, just previous to dumping the charge-car. In
the side walls of the shaft are iron door-frames, ordinarily bricked
up, but giving access to the shaft for repairs or barring out without
interfering with the movement of the charge-car. Extending across the
shaft, about 18 in. above the normal stock line, are three A-shaped
cast-iron deflectors, dividing the area of the shaft into four equal
rectangles.
The general arrangement of the plant is shown in Fig. 4. From the
charge-car pit there extends an inclined trestle, on an angle of 17
deg. to the charge-floor level, in line with the battery of furnaces.
The gage of the track is approximately equal to the length of the
furnaces at the top. The charge-car, actuated by a steel tail-rope,
moves sideways on this track from the charging-pit to any furnace
in the battery. The hoisting drums are located at the crest of the
incline, inside of the furnace building. At the far end of the latter
there is a tightener sheave, with a weight to keep proper tension on
the tail-rope. The charge-car has a capacity of 5 tons. It has an
A-shape bottom, and is so arranged that one attendant can quickly trip
the bolt and discharge the car.
[Illustration: FIG. 4.—Pueblo System. Longitudinal vertical section
through incline.]
While the car is making its trip the charge-wheelers are filling their
buggies, working in pairs, each man weighing up a halfcharge of a
particular ingredient. They then separate, each taking his proper place
in the line of wheelers on either side. When the car has returned, the
wheelers successively discharge their buggies into opposite ends of
the car. The coke is added last, to avoid crushing. The system is not
strictly economical of labor, since the wheelers, who must always be
ready for their car, have to wait for its return, which necessitates
more wheelers than would otherwise be required. Figs. 5, 6 and 7 show
the car.
[Illustration: FIG. 5.—Pueblo Charge-car. (Side elevation.)]
A vertical section through the car filled by dumping from the two ends
will show an arrangement of coarse and fine, which is far from regular.
Analyzing its structure, we shall find a conical pile near each end,
with a valley between them, in which coarse ore will predominate. The
deflectors in the furnace, previously referred to, serve to scatter
the fines as the charge is dropped in. Without them the feeding of the
furnace would be a failure; with them it is successful, though not so
completely as might be, the furnaces having a tendency to run with hot
tops. With the battery of seven furnaces, each smelting an average of
100 tons of ore per day, the saving, as compared with hand-feeding,
was $63 per day, or 9c. per ton of ore, this including cost of steam,
but not wear and tear on the machinery. This is distinctly a maximum
figure; with fewer furnaces the fixed charges of the mechanical feed
would soon increase the cost per ton to such a figure that the two
systems would be about equal in economy.
[Illustration: FIG. 6.—Pueblo Charge-car. (Plan.)]
[Illustration: FIG. 7.—Pueblo Charge-car. (End elevation.)]
_East Helena System._—This was introduced at the East Helena plant of
the United Smelting and Refining Company by H. W. Hixon. The plant
comprised four lead furnaces, each 48 × 136 in., with a 21 ft. smelting
column. They were all open-top furnaces, fed through a slot over the
center, the gases being taken off below the floor. They were capable of
smelting about 180 tons of charge (ore and flux) per 24 hours, using
a blast of 30 to 48 oz., furnished by two Allis duplex, horizontal,
piston blowers, air-cylinders 36 in. diam., 42 in. stroke, belted
from electric motors. The Hixon feed was designed to meet existing
conditions, without irrevocably cutting off convenient return to
hand feeding in case of an emergency. As shown in Fig. 9 there is a
track-way at right angles to the line of furnaces. The car hoisted up
the incline is landed on a transfer carriage, on which, after detaching
the cable, it can be moved over the tops of the furnaces by means of
a tail-rope system. The gage of the charge-car is 4 ft. 9 in.; of
the transfer carriage, 11 ft. 8 in. A switch at the lower end of the
incline permits two charge-cars to be employed, one being filled while
the other is making the trip. In sending down the empty car a hand
winch is necessary to start it from the transfer carriage. Figs. 10 and
11 show the charge-car; Fig. 12 the transfer carriage.
[Illustration: FIG. 8.—Pueblo System. (Sectional diagrams of furnace
top.)]
The charge-car is 10 × 4 × 3.5 ft., and has capacity for 6 tons of ore,
flux, slag and fuel, the total of ore and flux being usually 8800 lb.
Its bottom is flat, consisting of two doors, hinged along the sides
and kept closed by means of chains wound about a longitudinal windlass
on top of the car. The charging pits are decked with iron plates,
leaving a slot along the center of each car exactly like the slot in
the furnace top. The loaded ore-buggies are taken from the wheelers by
two men, who carefully distribute the contents of each buggy along the
whole length of the charge-car by dragging it along the slot while in
the act of dumping. Each buggy contains but one ingredient; they follow
one another in a prescribed order, so as to secure thin layers in the
charge-car. The coke is divided into three or more layers.
[Illustration: FIG. 9.—East Helena System. (Vert-longitudinal section
and plan of incline.)]
[Illustration: FIG. 10.—East Helena Charge-car. (Side elevation.)]
The first few trials of this device were not satisfactory. The furnaces
quickly showed over-fire, and decreased lead output, which would not
yield to any remedy except a return to hand feeding. The total charge
being dropped in the center of the furnace, a central core of fines
was produced, the lumps tending to roll toward the walls. This wrong
tendency was emphasized by the presence of the chains supporting
the bottom of the charge-car. On unwinding them to dump the car,
the doors were prevented from dropping by the wedging of the chains
in the charge, which in turn arched itself more or less against the
sides of the car; hence the doors opened but slowly, and often had to
be assisted by an attendant with a bar. In consequence of this slow
opening, considerable fine ore sifted out first and formed a ridge in
the center of the furnace, from the slopes of which the coarser part of
the charge, the last to fall, naturally rolled toward the sides. This
fact, determined during a visit of the writer in April, 1899, proved
to be the key to the situation. The attendant operating the tail-rope
mechanism was instructed to move the transfer carriage rapidly backward
and forward over the slot while the first one-third or one-half of
the charge was dropping, and during the rest of the discharge to let
the car stand directly over the slot and permit the coarser material
to fall in the center of the furnace. Two piles of comparatively fine
material were thus left on the charge-floor, one on each side of the
slot. These were subsequently fed in by hand, with instructions to
throw the material well to the sides of the furnace.
[Illustration: FIG. 11.—East Helena Charge-car. (Plan.)]
The furnaces were running very hot on top when this modified procedure
was begun. In a few hours the over-fire had disappeared; the lead
output was increasing; and the furnaces were running normally. This was
done about May 1, 1899, and from that time until about February 20,
1900, the Hixon feed, as modified above, was continuously in operation.
In October, 1898, with three furnaces in operation and hand feeding,
the labor cost per furnace was $42.06 per day; in October, 1899, with
the same number of furnaces and mechanical feeding, it was $41 per day,
the saving being only 0.6c. per ton of charge.
[Illustration: FIG. 12.—East Helena Charge-car and Transfer Carriage.
(Elevation.)]
[Illustration: FIG. 13.—East Helena System, with spreader and curtains.
(Experimental form.)]
_Dwight Spreader and Curtain._—In January, 1900, the writer again
had occasion to visit the East Helena plant, to investigate why a
certain cheap local coke could not be used successfully instead of
expensive Eastern coke. Strange as it may seem, the peculiar behavior
of the cokes was traced to improper feeding of the furnaces. Further
study of the mechanical feeding system, then in operation for nine
months, showed that it was far from perfect, and it appeared desirable
to design a spreader which would properly distribute the material
discharged from the Hixon car and dispense with hand feeding entirely.
An experimental construction was arranged, as shown in Fig. 13. The
flanged cast-iron plates around the feeding slot were pushed back and
a roof-shaped spreader, with slopes of 45 deg., was set in the gap,
leaving openings about 8 in. wide on each side. The plan provided for
two iron curtains to be hung, one on each side of the spreader, and so
adjusted that the fine ore sliding down the spreader would clear the
edge of the curtain and shoot toward the sides of the furnace, while
the coarse ore would strike the curtain and rebound toward the center
of the furnace. The classification effected in this manner was capable
of adjustment by raising or lowering the curtain. This arrangement was
found to work surprisingly well. The first furnace equipped with it
immediately showed improvement. It averaged better in speed, with lower
blast, lower lead in slag and matte, and better bullion output than
the other furnaces operating under the old system. The success of the
spreader and curtain being established, the furnaces were provided with
permanent constructions, the only modifications being that the ridge of
the spreader was lowered to correspond with the level of the floor and
the curtains were omitted, the feeding being apparently satisfactory
without their aid. In their absence, the lowering of the spreader was a
proper step, as it distributed the material fully as well, and caused
less abrasion of the walls. The final form is shown approximately
in Fig. 14. It has given complete satisfaction at East Helena since
February, 1900, and has been adopted as the basis for the mechanical
feeding device in the new plant of the American Smelting and Refining
Company at Salt Lake, Utah.
[Illustration: FIG. 14.—East Helena System. (Final form, approximate.)]
_Comparison of Systems._—In mechanical design the Pueblo system
is better than the East Helena, being simpler in construction and
operation. No time is lost in attaching and changing cables, operating
transfer carriage, etc. In both systems the track runs directly over
the tops of the furnaces, and this is an inconvenience when furnace
repairs are under way. The Pueblo car is the simpler, and makes the
round trip in about half the time of a car at East Helena, so the two
cars of the latter do not make much difference in this respect. The
system of filling the charge-car at Pueblo is also the quicker. It may
be estimated roughly that per ton of capacity it takes 2.5 to 3 times
as long to fill the East Helena car; and this means longer waiting on
the part of the wheelers, and consequently greater cost of moving the
material, representing probably 7 or 8c., in favor of Pueblo, per ton
of charge handled. However, both systems are wasteful of labor. As to
furnace results, it is believed that the better distribution of the
charge in the East Helena system leads to greatly increased regularity
of furnace running, less tendency to over-fire, some economy in fuel,
less accretions on the furnace walls and larger metal savings. If the
half of these conclusions are true, the difference of 7 or 8c. per ton
in favor of the Pueblo system, which can be traced almost entirely
to the cost of filling the charge-car, sinks into insignificance
in comparison with the important advantages of having the furnaces
uniformly and correctly fed.
_True Function of the Charge-Car._—The radically essential feature of a
mechanical feeding device is that part which automatically distributes
the material in the furnace, whatever approximate means may have been
used to effect the delivery.
Taking a hasty review of the numerous feeding devices that have
been tried in lead-smelting practice, we cannot but remark the fact
that those which depended upon dumping the charge into the furnace
from small buggies or barrows failed generally to secure a proper
classification and distribution of coarse and fine, and, consequently,
were abandoned as unsuccessful, while the adoption of the idea of the
charge-car for transporting the material to the furnace in large units
seems to have been coincident with a successful outcome. It is natural
enough, therefore, that the car should be regarded by many as the vital
feature. This view of the question is not, however, in accordance
with the true perspective of the facts, and merely limits the field
of application in an entirely unnecessary way. It must be apparent
that the essential function of the charge-car is cheap and convenient
transportation. The distribution of the charge is an entirely different
matter, in which, however, the charge-car may be made to assist, as
in the Pueblo system; or entirely distinct and special means may be
employed for the distribution, as in the East Helena system.
To follow the argument to its conclusion, let us imagine for the moment
that the East Helena plant were arranged on the terrace system, with
the furnace tops on a level with the floor of the ore-bins. Certain
precautions being observed, the spreader would give as good results
with small units of charge delivered by buggies as it now does with the
large units delivered by the charge-car, and the expense of delivery
to the furnaces would be practically no more than it now is to the
charge-car pit. The furnace top would, of course, have to be arranged
so that the buggies, in discharging, could be drawn along the slot,
so as to give the necessary longitudinal distribution parallel to the
furnace walls, just as is now done in filling the charge-car. The ends
of the spreader, if built like a hipped roof, would secure proper
feeding of the front and back.
Thus, by eliminating the charge-car, and with it the necessity for
powerful hoisting machinery, with its expensive repairs and operating
costs, we may greatly simplify the problem of mechanical feeding, and
open the way for the adoption of successful automatic feeding in many
existing plants where it is now considered impracticable.
COST OF SMELTING AND REFINING
BY MALVERN W. ILES
(August 18, 1900)
In the technical literature of lead smelting there is a lamentable lack
of data on the subject of costs. The majority of writers consider that
they have fulfilled their duties if they discuss in full detail the
chemical and engineering sides of the subject, leaving the industrial
consideration of cost to be wrought out by experience. When an engineer
or metallurgist collects data on the costs involved in the various
smelting operations, he generally hesitates to give this special
information to the public, as he regards it as private, or reserves it
as stock in trade to be held for his own use.
The following tables of cost have been compiled from actual results
of smelting and refining at the Globe works, Denver, Colo., and are
offered in the hope that they will prove a valuable addition to the
literature of lead smelting. These results are offered tentatively,
and, while true for the periods stated, they require considerable
adjustment to meet the smelting conditions of the present time.
COST OF HAND-ROASTING PER TON (2000 LB.) OF ORE
1887 $3.975
1888 4.280
1889 4.120
1890 3.531
1891 3.530
1892
1893
1894 3.429
1895 2.806
1896 2.840
1897 2.740
1898 2.620
At first the roasting was done mainly by hand roasters; later two
Brown-O’Harra mechanical furnaces were used, and the cost was reduced,
but not to the extent usually conceded to this type of furnace, as the
large amount of repairs and the consequent loss of time diminished
the apparent gain due to greater output. The figures quoted above may
be considered somewhat higher than the average, as the roasters were
charged in proportion with expenses of general management, office, etc.
In viewing the yearly reduction of costs one must take into
consideration many changes in the furnace construction and working, as
well as the items of labor, fuel, etc. From 1887 to 1899 the principal
changes in the construction of the hand-roasting furnaces consisted
in an increase of width, 2 ft., which allowed an addition of 200 lb.
to each ore charge, and corresponded to a total increase per furnace
of 1200 lb. in 24 hours. In the working of the charge an important
change was made in the condition of the product. Formerly the material
was fused in the fusion-box and drawn from the furnace in a fused or
slagged condition; and while this gave an excellent material for the
subsequent treatment in the shaft furnace in that there was very little
dusting of the charge, and a considerable increase in the output of the
furnace, the disadvantages of large losses of lead and silver greatly
over-balanced the advantages, and called for an entire abandonment of
the fusion-box. As a result of experience it was found that the best
condition of product is a semi-fused or sintered state, in which the
particles of roasted ore have been compressed by pounding the material,
which has been drawn into the slag pots, with a heavy iron disk. The
amount of “fines” under these conditions is quite small and depends
upon the percentage of lead in the ore, the degree of heat employed,
and the extent of the compression.
The total cost was partly reduced from the lessened labor cost
following the financial disturbance of 1893, and partly from the
reduction in the fuel cost, the former expensive lump coal being
replaced by the slack coals from southern Colorado.
The comparison of the cost of labor by the two methods shows a gain of
54c. a ton in favor of the mechanical furnaces. However, I consider
that this gain is a costly one, and is more than offset by the large
amount of high-grade fuel required, and the expense of repairs not
shown in the following table. Indeed, I believe that at the end of five
or ten years the average cost of roasting per ton by the hand roasters
will be even smaller than by these mechanical roasters.
To illustrate the details of roasting cost and to furnish a comparison
of the hand roasters and mechanical furnaces, the following table has
been prepared:
DETAILS OF AVERAGE MONTHLY COST FOR 1898 OF HAND ROASTERS AND
MECHANICAL FURNACES
───────────┬────────┬───────┬─────────────────────┬─────────────────────
│ │ │ HAND ROASTERS │ BROWN-O’HARRA
│ │ │ │ MECHANICAL FURNACES
│ TOTAL │ TONS ├──────┬──────┬───────┼──────┬──────┬───────
Month │ TONS │ROASTED│LABOR │ COAL │GENERAL│LABOR │COAL │GENERAL
│ROASTED │PER DAY│ $ │ $ │EXPENSE│ $ │ $ │EXPENSE
│ │ │ │ │ $ │ │ │ $
───────────┼────────┼───────┼──────┼──────┼───────┼──────┼──────┼───────
January │ 5,691 │ 184 │ 1.47 │ 0.53 │ 0.80 │ 0.92 │ 0.80 │ 1.32
February │ 5,677 │ 203 │ 1.44 │ 0.44 │ 0.99 │ 0.72 │ 0.58 │ 1.01
March │ 5,821 │ 188 │ 1.51 │ 0.53 │ 0.64 │ 0.76 │ 0.64 │ 0.62
April │ 5,472 │ 182 │ 1.47 │ 0.47 │ 0.71 │ 0.80 │ 0.69 │ 0.87
May │ 5,444 │ 176 │ 1.55 │ 0.51 │ 0.84 │ 0.80 │ 0.69 │ 0.81
June │ 4,859 │ 162 │ 1.58 │ 0.48 │ 0.71 │ 0.90 │ 0.68 │ 1.17
July │ 5,691 │ 184 │ 1.59 │ 0.48 │ 0.75 │ 0.72 │ 0.56 │ 0.64
August │ 5,910 │ 191 │ 1.55 │ 0.46 │ 0.83 │ 0.72 │ 0.55 │ 0.75
September │ 5,677 │ 189 │ 1.55 │ 0.45 │ 0.74 │ 0.73 │ 0.55 │ 0.67
October │ 6,254 │ 202 │ 1.48 │ 0.49 │ 0.72 │ 0.65 │ 0.50 │ 0.60
November │ 6,291 │ 213 │ 1.42 │ 0.47 │ 0.80 │ 0.66 │ 0.53 │ 0.70
December │ 5,874 │ 198 │ 1.45 │ 0.48 │ 0.78 │ 0.79 │ 0.63 │ 0.81
├────────┼───────┼──────┼──────┼───────┼──────┼──────┼───────
Average │ │ │ 1.50 │ 0.48 │ 0.77 │ 0.76 │ 0.62 │ 0.83
Total │ │ │ │ │ 2.75 │ │ │ 2.21
───────────┴────────┴───────┴──────┴──────┴───────┴──────┴──────┴───────
_Cost of Smelting._—The lead-ore mixtures of the United States, in
addition to lead, contain gold, silver and generally copper, and are
treated to save these metals. The total cost of smelting is made up of
a large number of items. The questions of locality and transportation,
fuel, fluxes and labor are the principal factors, to which must be
added the handling of the material to and from the furnace; the
furnace itself, its size, shape, and method of smelting, the volume
and pressure of blast, etc. The following table of costs, from 1887 to
1898, shows in a general way the great advance that has been made in
the development of smelting, and the consequent reduction in cost per
ton of ore treated:
AVERAGE COST OF SMELTING, PER TON
1887 $4.644
1888 4.530
1889 4.480
1890 4.374
1891 4.170
1892 4.906
1893 3.375
1894 3.029
1895 2.786
1896 2.750
1897 2.520
1898 2.260
In connection with this table of smelting cost should be considered the
changes developed during the interval 1887-1889, outlined as follows:
CONDITIONS OF SMELTING IN 1886 AND 1899 CONTRASTED TO SHOW THE PROGRESS
OF DEVELOPMENT
────┬───────────────┬────────────┬───────────────┬─────────────┐
│AREA OF FURNACE│ HEIGHT OF │BLAST PRESSURE,│ FORE HEARTH │
│ AT TUYERES, │CHARGE FROM │ LB. PER │CAPACITY, CU.│
│ IN. │TUYERES, FT.│ SQ. IN. │ FT. │
────┼───────────────┼────────────┼───────────────┼─────────────┤
1886│ 30 × 100 │ 11 │ 1 │ 6 │
│ │ │ │ │
│ │ │ │ │
1899│ 42 × 140 │ 16 │ 3 to 4 │ 128 │
│ │ │ │ │
────┴───────────────┴────────────┴───────────────┴─────────────┘
────┬────────────┬────────┬───────────────┬───────────────┐
│ SLAG │ FUEL │ SLAG REMOVED, │MATTE REMOVED, │
│ SETTLED │ │ LB. PER TRIP │ LB. PER │
────┼────────────┼────────┼───────────────┼───────────────┤
1886│ │ │ │ TRIP │
│ In pots │Charcoal│ By hand │ By hand │
│ │ │ 280 │ 200 │
1899│ │ │ │ │
│In furnaces │ Coke │ By locomotive │ By horse │
│ │ │ 3000-6000 │ 2000-3000 │
────┴────────────┴────────┴───────────────┴───────────────┘
I believe that there is room for further improvement in the
substitution of mechanical transportation within the works for hand
labor, and that the fuel cost can be materially reduced by replacing
the coke, which at present contains 16 to 22 per cent. of ash, by a
fuel of purer and better quality.
_Cost of Refining by the Parkes Process._—In general it may be stated
that the average cost of refining base bullion is from $3 to $5 a
ton. This amount is based on the cost of labor, spelter, coal, coke,
supplies, repairs and general expenses. When the additional items
of interest, expressage, brokerage and treatment of by-products are
considered, which go to make up the total refining cost, the amount may
be stated approximately as $10 per ton of bullion treated.
Variations in the cost occur from time to time, and are due to several
causes, principally the irregularity of the bullion supply and its
consequent effect on the work of the plant. When the amount of bullion
available for treatment is small, the plant cannot be run to its
maximum capacity, and the cost per ton will naturally be increased. To
illustrate this variation, the average cost per ton of base bullion
refined during nine months in 1893 was:
January, $4.864; February, $5.789; March, $5.024; April, $3.915; May,
$5.094; June, $4.168; July, $4.231; August, $4.216; September, $5.299.
The yearly variation shows but little change, as the average cost per
ton was for 1893, $4.75; for 1894, $3.99; for 1895, $4.21; for 1896,
$3.90. In considering the total cost of refining, the additional
factors of interest, expressage, parting, brokerage, and reworking of
by-products must be considered. As the doré silver is treated at the
works or elsewhere, so will the total cost be less or greater. The
following table gives the cost in detail, when the parting is done at
the same works:
AVERAGE MONTHLY COST OF REFINING PER TON OF BULLION TREATED
─────────────────────┬────────────┬────────────┬────────────┬─────────
ITEMS │ 1895 │ 1895 │ 1896 │ AVERAGE
│JAN. TO JULY│JULY TO DEC.│JAN. TO JULY│
─────────────────────┼────────────┼────────────┼────────────┼─────────
Labor │ $2.351 │ $1.718 │ $1.836 │ $1.968
Spelter │ 0.757 │ 0.840 │ 0.987 │ 0.861
Coal │ 0.585 │ 0.442 │ 0.461 │ 0.496
Coke │ 0.634 │ 0.418 │ 0.511 │ 0.521
Supplies, repairs and│ │ │ │
general expenses │ 0.343 │ 0.273 │ 0.252 │ 0.289
Interest │ 1.808 │ 1.075 │ 1.070 │ 1.317
Expressage │ 1.360 │ 1.015 │ 0.882 │ 1.085
Parting and brokerage│ 2.483 │ 2.084 │ 1.796 │ 2.121
Reworking by-products│ 1.567 │ 1.286 │ 1.625 │ 1.492
├────────────┼────────────┼────────────┼─────────
Totals │ $11.888 │ $9.151 │ $9.420 │ $10.151
Tons bullion refined │5,511.58 │9,249.07 │10,103.43 │8,287.99
─────────────────────┴────────────┴────────────┴────────────┴─────────
An analysis of the different items of cost is important, and a brief
summary is given below.
_Labor and Attendance._—The cost for this item varies but little from
year to year, and its reduction depends, for the most part, on a larger
yield per man rather than on a reduction of wages. If a man at the same
or slightly increased cost can give a larger output, so will the labor
cost per ton be diminished. This result is accomplished by enlarging
the furnace capacity and by using appliances which will handle the
bullion and its products in an easier and quicker manner. The small
size of the furnaces, settlers and retorts used at modern refineries is
open to criticism; I believe that great improvement can be made in this
direction.
_Spelter._—The cost of this item varies with the market conditions,
and will probably be changed but little in the future, as the amount
necessary per ton of bullion seems to be fixed.
_Coal._—The amount required per ton of bullion is fairly constant, and
while lessened cost for fuel may be attained by the substitution of oil
or gaseous fuel, the fuel cost in comparison with the aggregate cost is
very small, and leaves little opportunity for improvement in this line.
_Supplies._—This item includes brooms, shovels, wheelbarrows, etc., and
the amount is small and fairly constant from year to year.
_Repairs._—This item is quite small in works properly constructed;
and in this connection I wish to call particular attention to the
floor covering, which should be made of cast-iron plates from 1.5 to
2 in. thick, and placed on a 2 to 3 in. layer of sand spread over the
well-tamped and leveled ground. The constant patching of brick floors
is not only an annoyance, but is costly from the additional labor
required. Furthermore, a brick floor does not permit a close saving of
the metallic scrap material.
It will be found economical in the long run to protect all exposed
brickwork of furnaces or kettles with sheet iron.
In the construction of the refinery building I should advise brick
walls except at the end or side, where there is the greatest likelihood
of future extension; here corrugated iron may be used. The roof should
not be made of corrugated iron, as condensed or leakage water is liable
to collect and drop on those places where water should be scrupulously
avoided. The presence of water in a mold at the time of casting, even
though small in amount, will cause explosions and will scatter the
molten lead, endangering the workmen.
The item of repair for the ordinary corrugated iron roof may be
diminished by constructing it of 1 in. boards with intervening spaces
of half an inch, the whole overlaid with tarred felt, and covered with
sheets of iron at least No. 27 B. W. G., painted with graphite paint
and joined together with parallel rows of ribbed crimped iron.
_General Expenses._—This item is generally constant, and calls for no
special comment.
_Interest._—This important item is, as a rule, considerable, as the
stock of bullion and other gold-and silver-bearing material is quite
large. For this reason special attention should be given to prevent
the accumulation of stock or by-products. The occasional necessity of
additional capital to run the business should preferably be met by an
increase of working capital, rather than by a direct loan.
_Expressage._—This item, as a rule, is large, and should be taken into
consideration in the original plans for the location of the refining
works.
_Parting._—The item of parting and brokerage is the largest of the
refinery costs, and for obvious reasons a modern smelting plant should
have a parting plant under its own control.
_The Working of the By-Products._—This constitutes a large item of
cost, and considerable attention should be devoted to the improvement
of present methods, which seem faulty, slow and expensive.
_Summary._—The items of smaller cost with their respective amounts per
ton of base bullion treated are: Spelter, $0.85; coal, $0.50; coke,
$0.50; supplies, repairs and general expenses, $0.35; total, $2.10. It
is doubtful whether much improvement can be made in the reduction of
these costs.
The items of larger cost are: Labor, $2; interest, $1.32; expressage,
$1.10; parting and brokerage, $2; reworking by-products, $1.50; total,
$7.92. The general manager usually attends to the items of interest,
expressage and brokerage, leaving the questions of labor and working of
by-products to the metallurgist.
The cost quoted for smelting practice, as employed at Denver, will
differ necessarily from those at other localities, where the cost of
labor, freight rates on spelter, fuel, etc., are changed. Refining
can doubtless be done at a lower cost at points along the Mississippi
River, and even more so at cities on the Atlantic seaboard, as Newark
or Perth Amboy, N. J.
The consolidation of many of the more important smelting plants of the
United States under one management will doubtless alter the figures of
cost given above, particularly as the interest cost there stated is at
the high rate of 10 per cent., a condition of affairs now changed to 5
per cent. Other factors have lessened the cost of refining; the bullion
produced at the present time is softer, or contains a smaller amount
of impurities, and admits of easier working with shorter time and less
labor. By proper management larger tonnages are turned out per man, and
the Howard stirrer and Howard press have simplified and cheapened the
working of the zinc skimmings. To illustrate the comparatively recent
conditions of cost I have compiled the following table for each month
of the year 1898:
COST OF REFINING DURING 1898, INCLUDING LABOR, SPELTER, COAL, COKE,
SUPPLIES, REPAIRS AND GENERAL EXPENSES.
January $3.59
February 3.28
March 3.26
April 3.59
May 3.38
June 3.56
July 3.65
August 3.54
September 3.35
October 3.45
November 3.20
December 3.56
Average cost during the year, $3.45.
It is understood, of course, that these figures do not include cost of
interest, expressage, parting, brokerage and reworking of by-products.
[Although this article refers to conditions in 1898, since which time
there have been improvements in practice, the latter have not been of
radical character and the figures given are fairly representative of
present conditions.—EDITOR.]
SMELTING ZINC RETORT RESIDUES[13]
BY E. M. JOHNSON
(March 22, 1906)
The following notes were taken from work done at the Cherokee
Lanyon Smelter Company, Gas, Kansas, in 1903. It was practically an
experiment. The furnace was only 36 × 90 in. at the crucible, with a
10 in. side bosh and a 6 in. end bosh. There were five tuyeres on each
side with a 3 in. opening. The side jackets measured 4.5 ft. × 18 in.
The distance from top of crucible to center of tuyeres was 11.5 in.
The blast was furnished by one No. 4½ Connellsville blower. The
furnace originally was only 11 ft. from the center of tuyeres to the
feed-floor, and had only been saving about 60 per cent. of the lead.
This loss of lead, however, was not entirely due to the low furnace.
As no provision had been made to separate the slag and matte, upon
assuming charge I raised the feed-floor 3 ft., thereby changing the
distance from the tuyere to top of furnace from 11 ft. to 14 ft. Matte
settlers were also installed. These two changes raised the percentage
of lead saved to 92, as shown by monthly statements. The furnace being
small, and a high percentage of zinc oxide on the charge, the campaigns
were naturally short. The longest run was about six weeks. This was
made on some residue that had been screened from the coarse coal, and
coke, and had weathered for several months. This particular residue
also carried about 10 per cent. lead. The more recent residue that had
not been screened and weathered, and was low in lead, did not work so
well. Although these residues consisted of a large proportion of coal
and coke, it seemed impossible to reduce the percentage of good lump
coke on the charge lower than 12.5 or 13 per cent. At the same time the
reducing power of the residue was strong, and with the normal amount of
coke caused some trouble in the crucible.
When residue containing semi-anthracite coal was smelted, the saving
in lead dropped, and the fire went to the top of the furnace, burning
with a blue flame, thereby necessitating the reduction of this class of
material. This residue had been screened through a five-mesh screen,
and wet down in layers, becoming so hard that it had to be blasted.
The low saving of lead with this class of material was a surprise,
as it has been claimed that the substitution of part of the fuel by
anthracite coal did not affect the metallurgical operations of the
furnace.
The slag was quite liquid and flowed very well at all times. However,
there was a marked variation in the amount at different tappings. This,
I am satisfied, was not due to irregular work on the furnace, but may
be accounted for in the following manner. The residue (not screened or
weathered to any extent), consisting approximately of one-half coal
and coke, was very bulky, and while there was about 35 per cent. of it
on the charge by weight, there was over 50 per cent. of it by bulk,
not including slag and coke. In feeding, therefore, it was a difficult
matter to mix the whole of it with the charge. Several different ways
of feeding the furnace were tried. The one giving the most satisfactory
results was to feed nearly all of the residue along the center of the
furnace, in connection with the lime-rock, coarse ore and coarse iron
ore, and the fine and easy smelting ores along the sides. The slag was
spread uniformly over the whole furnace, while the sides were favored
with the coke. The charge would drop several inches at a time, going
down a little faster in the center than on the sides.
It is possible that a small proportion of the residue in connection
with the easy smelting, leady, neutral ore, iron ore and lime-rock
formed the type of slag marked No. 1.
───┬───────┬──────┬─────┬──────┬─────┬─────┬────
│ SiO₂ │ FeO │ MnO │ CaO │ ZnO │ Pb │ Ag
───┼───────┼──────┼─────┼──────┼─────┼─────┼────
1 │ 33.7 │ 34.1 │ 1.0 │ 16.5 │ 7.5 │ 0.9 │ 0.7
2 │ 31.0 │ 36.1 │ 1.2 │ 16.0 │ 9.6 │ 1.3 │
───┴───────┴──────┴─────┴──────┴─────┴─────┴────
This being tapped with a good flow of slag, the charge would drop,
bringing a proportionately large amount of residue in the fusion zone
which formed the type of slag marked No. 2. There was also a marked
variation in the slag-shells from different pots. The above cited
irregularities of course exist to a certain extent in any blast furnace.
AVERAGE ANALYSIS OF MATERIALS SMELTED
NAME ROW NAME ROW
Mo. iron ore A Roasted matte[15] F
Lime rock B Barrings G
Mo. galena C Coke ash H
Av. of beds D Coke[16] J
Residue[14] E
────┬──────┬─────┬────┬────┬────┬─────┬─────┬────┬────┬───┬────┬────
│ SiO₂ │ FeO │CaO │MgO │ZnO │Al₂O₃ │Fe₂O₃ │ S │ Pb │Cu │ Ag │ Au
────┼──────┼─────┼────┼────┼────┼─────┼─────┼────┼────┼───┼────┼────
A │ 10.0 │ 65.0│ │ │ │ │ │ │ │ │ │
B │ 1.5 │ │52.0│ │ │ │ │ │ │ │ │
C │ 1.5 │ 2.4│ │ │ 9.5│ │ │11.0│74.0│ │ │
D │ 50.8 │ 16.2│ │ │ 4.6│ │ │ 3.3│ 9.1│ │ │
E │ 10.5 │ 38.5│ │ │18.0│ │ │ 4.8│ 2.2│1.0│10.0│0.03
F │ 9.0 │ 48.0│ 3.0│ │10.0│ │ │ 4.0│ 9.9│3.0│21.0│0.06
G │ 18.8 │ 24.4│ 5.0│ │14.5│ │ │ 6.0│25.4│ │13.0│0.07
H │ 27.0 │ │14.9│ 4.5│ │ 19.7│ 31.6│ │ │ │ │
│ H₂O │ V.M.│F.C.│ Ash│ S │ │ │ │ │ │ │
J │ 1.2 │ 2.3 │85.7│11.1│ 0.9│ │ │ │ │ │ │
─────┴──────┴─────┴────┴────┴────┴─────┴─────┴────┴────┴───┴────┴────
ANALYSIS OF BULLION, SLAG AND MATTE PRODUCED
│/-BULLION-\ /—————————————SLAG———————————————-\/————-MATTE————-\
│ Ag │ Au │SiO₂ │FeO │MnO│CaO │ZnO │ Pb │ Ag │ Ag │ Au │Pb │Cu
├──────┼────┼─────┼────┼───┼────┼────┼────┼────┼────┼────┼───┼───
Feb. │ 90.0 │1.15│31.2 │35.9│1.0│14.5│10.3│0.88│0.98│19.0│0.04│8.7│1.5
March│ 93.1 │1.63│31.3 │37.2│1.0│13.9│11.1│0.71│1.30│21.0│0.06│8.0│2.5
April│104.3 │1.59│29.8 │37.7│2.7│13.9│11.4│0.52│1.40│23.0│0.07│7.0│3.5
May │ 90.0 │1.24│30.0 │37.3│2.2│14.1│ 9.3│0.86│1.10│25.4│0.07│5.1│4.0
July │ 78.7 │1.00│32.2 │37.4│1.0│13.9│ 9.8│0.50│1.15│21.3│0.03│8.9│4.0
Aug. │ 90.8 │1.21│31.2 │37.1 1.7│13.7│ 9.6│1.10│1.60│23.1│0.08│9.8│3.0
Sept.│ 65.3 │2.58│32.0 │39.7│0.8│14.1│ 8.1│0.80│1.30│18.6│0.06│7.6│2.3
├──────┼────┼─────┼────┼───┼────┼────┼────┼────┼────┼────┼───┼───
Avge.│ 87.5 │1.49│31.1 │37.5│1.5│14.1│10.0│0.77│1.26│21.6│0.06│7.8│3.0
─────┴──────┴────┴─────┴────┴───┴────┴────┴────┴────┴────┴────┴───┴───
MONTHLY RECORD OF FURNACE OPERATIONS
─────────┬──────┬───────┬─────────┬─────────┬─────────┬─────────┐
│BLAST │ TONS │PER CENT.│PER CENT.│PER CENT.│PER CENT.│
│OUNCES│ PER │ PB. ON │ COKE ON │ SLAG ON │ S ON │
│ │ F.D. │ CHARGE │ CHARGE │ CHARGE │ CHARGE │
─────────┼──────┼───────┼─────────┼─────────┼─────────┼─────────┤
Feb. │ 21 │ 42.5 │ 9.0 │ 12.0 │ 30.0 │ 3.7 │
March │ 21 │ 44.8 │ 9.7 │ 13.5 │ 37.0 │ 4.0 │
April │ 21 │ 43.7 │ 9.0 │ 13.5 │ 35.0 │ 4.3 │
May │ 21 │ 49.4 │ 10.0 │ 13.5 │ 30.0 │ 3.5 │
July │ 17 │ 41.0 │ 9.8 │ 12.5 │ 34.0 │ 3.8 │
August │ 18 │ 47.0 │ 9.3 │ 13.0 │ 32.0 │ 3.7 │
Sept.[1
Read full text (200,001 characters)
Fields
| author | |
|---|---|
| language | English |
| chars | 625993 |
| source_url | https://www.gutenberg.org/ebooks/63784 |
Cite this record
MLA
"Lead Smelting and Refining, With Some Notes on Lead Mining." Project Gutenberg, n.d., https://gutenberg.go-v.org/record/63784.
Chicago
"Lead Smelting and Refining, With Some Notes on Lead Mining." Project Gutenberg. n.d.. https://gutenberg.go-v.org/record/63784.
APA
Project Gutenberg. (n.d.). Lead Smelting and Refining, With Some Notes on Lead Mining. https://gutenberg.go-v.org/record/63784