gutenberg.go-v.org

A treatise on the origin, progress, prevention, and cure of dry rot in timber

The Project Gutenberg eBook of A treatise on the origin, progress, prevention, and cure of dry rot in timber This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: A treatise on the origin, progress, prevention, and cure of dry rot in timber with remarks on the means of preserving wood from destruction by sea worms, beetles, ants, etc. Author: Thomas Allen Britton Release date: September 13, 2017 [eBook #55541] Most recently updated: October 23, 2024 Language: English Other information and formats: www.gutenberg.org/ebooks/55541 Credits: Produced by Chris Curnow and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) *** START

source: Project Gutenberglicence: Public domain (per item)database: /home/dbs/gutenberg.dbmode: tablerecords: 544887 (max_rowid)citation: https://www.gutenberg.org/

The Project Gutenberg eBook of A treatise on the origin, progress, prevention, and cure of dry rot in timber

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: A treatise on the origin, progress, prevention, and cure of dry rot in timber
with remarks on the means of preserving wood from destruction by sea worms, beetles, ants, etc.

Author: Thomas Allen Britton

Release date: September 13, 2017 [eBook #55541]
Most recently updated: October 23, 2024

Language: English

Other information and formats: www.gutenberg.org/ebooks/55541

Credits: Produced by Chris Curnow and the Online Distributed
Proofreading Team at http://www.pgdp.net (This file was
produced from images generously made available by The
Internet Archive)

*** START OF THE PROJECT GUTENBERG EBOOK A TREATISE ON THE ORIGIN, PROGRESS, PREVENTION, AND CURE OF DRY ROT IN TIMBER ***

[Illustration:

SKETCH OF DRY ROT FUNGUS

_On basement floor joist in house, at Greenwich, near London Feb 1875._

END OF JOIST

_Crumbled into fine red powder, with slight rubbing._

TOP OF JOIST.

_Portion of fungus near the edge was torn away on removal of floor
boards, the undersides of which were covered with fungus, as well as the
sides of nearest joist 10ins. distant._

_Portion of fungus near the edge was torn away on removal of joist.
Fungus covered top and sides of sleeper joist._

_Colours of fungi. White, yellow, green, purple, and rusty red._]

A TREATISE
ON THE
ORIGIN, PROGRESS, PREVENTION, AND CURE
OF
DRY ROT IN TIMBER.

WITH REMARKS ON
THE MEANS OF PRESERVING WOOD FROM DESTRUCTION BY
SEA WORMS, BEETLES, ANTS, ETC.

BY
THOMAS ALLEN BRITTON,
LATE SURVEYOR TO THE METROPOLITAN BOARD OF WORKS, AND SILVER
MEDALLIST OF THE ROYAL INSTITUTE OF BRITISH ARCHITECTS IN 1854,
1856, AND 1870.

[Illustration]

LONDON:
E. & F. N. SPON, 48, CHARING CROSS.
NEW YORK: 446, BROOME STREET.
1875.

THIS VOLUME
IS
Dedicated to
GEORGE VULLIAMY, ESQ.,
VICE-PRESIDENT
OF THE
ROYAL INSTITUTE OF BRITISH ARCHITECTS;
AND
ARCHITECT
OF
THE METROPOLITAN BOARD OF WORKS;
AS A SLIGHT ACKNOWLEDGMENT
OF HIS
COUNSEL, SYMPATHY, AND FRIENDSHIP,
DURING MANY YEARS.

PREFACE.

In preparing this treatise on Dry Rot, the author has endeavoured
to place in as condensed a form as was consistent with the nature
of the subject, the knowledge and information dispersed through a
numerous collection of writers who have treated thereon; he has also
availed himself of the assistance of professional friends, builders,
timber-merchants, foremen and carpenters; and, by so doing, has been
enabled to record several instances of the progress and cure of dry
rot. He has consulted many valuable papers published during the last
thirty years, in the various professional journals in England, America,
France, and Germany, upon this important subject, and has also obtained
much useful information from the works of Evelyn, Nicholson, Tredgold
by Hurst, Papworth, Burnell, Blenkarn, and other English writers upon
timber; Silloway, of North America; Porcher, of South America; Du Hamel,
De Moray, and De Lapparent, of France; and several writers whose works
will be referred to.

It is many years since a separate and complete work on dry rot has been
published, and those who are desirous of inquiring into the matter are
frequently at a loss where to obtain any information. Existing works on
the subject are out of print, and although they can be seen at a few
professional institutes, they are beyond the reach of the general public.

It has been the aim of the author in preparing this treatise to give a
fair hearing to every patentee, and he has endeavoured to be as impartial
as possible in recording instances of failure and success. If he has
erred in any particular case, he will be happy, should this work reach a
second edition, to make any necessary correction.

The reader will probably find some things repeated in the course of the
work; this is in many cases unavoidable, and in some advisable; for if by
a little tautology important truths can be impressed upon the mind of the
reader, the author will feel that his labour in preparing this work has
not been altogether in vain.

Modern authorities have been relied upon in preference to ancient ones:
the following sentence, written by the late Sydney Smith, is quoted as a
reason for so doing:

“Those who come first (our ancestors) are the young people, and have the
least experience. We have added to their experience the experience of
many centuries; and, therefore, as far as experience goes, are wiser, and
more capable of forming an opinion than they were.”

20, LIMES GROVE, LEWISHAM,
_May 14th, 1875_.

CONTENTS.

CHAPTER I.

On the Nature and Properties of Timber Page 1

CHAPTER II.

On the Gradual Rise and Development of Dry Rot 14

CHAPTER III.

On Felling Timber 51

CHAPTER IV.

On Seasoning Timber by Natural Methods, viz. Hot and Cold Air;
Fresh and Salt Water; Vapour; Smoke; Steam; Boiling; Charring
and Scorching, &c. 63

CHAPTER V.

On Seasoning Timber by Patent Processes, &c. 105

CHAPTER VI.

On the Means of Preventing Dry Rot in Modern Houses 171

CHAPTER VII.

On the Means of Preservation of Wooden Bridges, Jetties, Piles,
Harbour Works, &c., from the Ravages of the _Teredo navalis_ and
other Sea-worms 203

CHAPTER VIII.

On the Destruction of Woodwork in Hot Climates by the _Termite_
or White Ant, Woodcutter, Carpenter Bee, &c.; and the Means of
Preventing the Same 240

CHAPTER IX.

On the Causes of Decay in Furniture, Wood Carvings, &c.; and the
Means of Preventing and Remedying the Effects of such Decay 262

CHAPTER X.

Summary of Curative Processes 283

CHAPTER XI.

General Remarks and Conclusion 288

INDEX 295

ILLUSTRATIONS.

DRY ROT ON FLOOR JOIST _Frontispiece_

_To face page_

TIMBER BEAMS--ROTTEN AT THE HEART 34

BALTIC MODES OF CUTTING DEALS 64

MR. KYAN’S TIMBER PRESERVING TANK 126

MESSRS. BETHELL AND CO.’S TIMBER PRESERVING APPARATUS 136

TIMBER PILES FROM BALACLAVA HARBOUR 208

DESTRUCTION OF TIMBER PILE BY TEREDO 212

SHELL AND CELL OF TEREDO NAVALIS 216

PILES, SOUTHEND PIER; LIMNORIA, &C. 220

CARPENTER BEES AT WORK 260

A TREATISE ON DRY ROT IN TIMBER.

CHAPTER I.

ON THE NATURE AND PROPERTIES OF TIMBER.

In considering the subject of Timber trees, we commence with their
Elementary Tissues, and first in order is the _Formative Fluid_, which
is the sole cause of production of every tissue found in trees. It
is semi-fluid, and semi-transparent, and in this condition is found
abundantly between the bark and the wood of all trees in early spring;
and thus separates those parts so as to permit the bundles of young wood
to pass down from the leaves, and thus enable the tree to grow. It is
under these conditions that the woodman strips the bark from trees which
are to be cut down, since then it does not adhere to the wood.

The first step in the formation of any tissue from the formative fluid
is the production of a solid structureless fabric called _Elementary
Membrane_, and a modification of that fabric termed _Elementary Fibre_.

The structures which are produced from the above-mentioned “raw
material” are very varied in appearance, and are called _Cellular
Tissues_, to signify that they are made up of hollow cells. The spaces
between the cells are called _Intercellular Spaces_, which are of vital
importance, as they contain air. _Woody fibre_ constitutes the mass of
the stems of our forest trees. Its peculiar characteristic is that of
great tenacity, and power of resistance, and for this its structure is
admirably adapted: it consists of bundles of very narrow fibres, with
tapering extremities, and is so placed from end to end, that the pointed
ends overlap each other. Each fibre is very short, and the partitions
which result from the apposition of the fibres, end to end, do not
interfere with the circulation through them. The tube is not composed
of simple thin membranes only; but in addition has a deposit within it,
which, without filling the tube, adds very greatly to the strength of
the fibre: an arrangement whereby the greatest strength and power of
resistance and elasticity shall be obtained; and, at the same time, the
functions of circulation uninterruptedly maintained. The strength is
mainly due to the shortness of each fibre, the connection by opposite
ends of many fibres, almost in one direct line, from the root upwards;
and lastly, to the deposit on the inner side of the membrane. The uses
of woody fibre are very varied and most important; it is the chief organ
of circulation in all wooded plants, and, for this purpose, pervades
the plant from the root to the branches. The current in this tissue
is directed upwards from the shoot, through the stem to the leaves,
and downwards from the leaves through the bark to the root. Thus, its
current has a twofold tendency; the ascending and chief one being for
the purpose of taking the raw, or what is called the _common sap_, from
the ground to be digested in the leaves, and the descending being devoted
to the removal from the leaves of the digested, or what is termed the
_proper sap_, to be applied to the purposes of the tree, and also of the
refuse matter to be carried to the roots, and thence thrown out into the
soil as a noxious material. The _proper sap_ differs considerably in
different trees; it is always less liquid, and contains a much greater
proportion of vegetable matter than the common sap. It is very probable
that trees of the same kind produce proper sap of different qualities in
different climates.

WOODY FIBRE may be considered the storehouse of the perfected secretions.
It is well known that as trees advance in life, the wood assumes a darker
colour, and more particularly that lying near to the centre of the stem.
This is due to the deposit of the perfected juices in the woody fibre at
that point; and where age has matured the tree, it is probable that the
woody fibre so employed is no longer fitted for the circulation of the
sap; and, also, that the perfected sap, when once deposited, does not
again join in the general circulation. The dark colour of the heart of
oak, as contrasted with oak of very recent growth, is an illustration
of this fact, as is also the deep colour which is met with in ebony and
rose-wood. Technically, the inner wood is called the heart-wood, and the
outer or younger wood the sap-wood. Of these, the former contains little
fluid, and no vegetable life, and, being the least liable to decay, is
therefore the most perfect wood; the latter is soft and perishable in
its nature, abounding in fermentable elements; thus affording the very
food for worms, whose destructive inroads hasten its natural tendency to
decay.

The proportion of sap-wood in different trees varies very much. Spanish
chestnut has a very small proportion of sap-wood, oak has more, and fir a
still larger proportion than oak; but the proportions vary according to
the situation and soil, and according to the age at which they have been
felled: for instance, the teak tree in Malabar, India, differs from teak
in Anamalai, South India. This subject has been very fully treated by Mr.
Patrick Williams, in his valuable work on Naval Timber.

WOODED STEMS are divided into two great and well-defined classes,
according to their internal conformation, viz. such as grow from without
(exogenous), and such as enlarge from within (endogenous). The former are
more common in cold, and the latter in hot climates.

EXOGENOUS STEMS.--On examining a section of a stem of an oak, or any
other of our forest trees, we observe the following parts: first, the
pith, or its remains in the centre; second, the bark on the outside;
third, a mass of wood between the two, broken up into portions by the
concentric deposition of the layers, and by a series of lines which
pass from the centre to the circumference. Thus, there are always pith,
bark, wood, and medullary rays. Each stem has two systems, the cellular
or horizontal, and the vascular or longitudinal, and the parts just
mentioned must belong to one or other of those systems. Thus, the pith,
medullary rays, and bark belong to the horizontal system; and the wood
constitutes the longitudinal system.

THE PITH occupies the centre of the stem, and remains throughout the
period of growth of some trees, as of the elder; or is abstracted after
a few years, as in the oak, and almost all large trees. In the latter
class of trees, there are some remains of the pith for many years after
the process of absorption has commenced, but at length no vestige can
be detected, and its position is known only by the central spot around
which the wood is placed in circles. In the old age of the tree the pith
frequently assumes a colour which it has obtained from the juices which
have been deposited. The connections of the pith are extremely important.
Firstly, it is in direct connection with every branch, and is the
structure which first conveys fluids to, and receives fluids from every
new leaf. It thence becomes the main organ of nutriment, and, at the same
time, the chief depository of the secretions. Secondly, it is in equally
direct and unbroken connection with the bark, through the medium of the
medullary rays; and so becomes the centre of all the movements of sap
which proceed in the horizontal system.

The mode in which the ultimate disappearance of the pith occurs has been
a matter of speculation. That the circulation in the heart-wood ceases
after a certain number of years, and that the connection between it and
the bark becomes broken, is proved by the fact that numbers of trees
may be found in tolerably vigorous growth within the bark, whereas at
the heart they are decayed and rotten. It appears clear that it is not
converted into wood, and there are facts against the opinion that it
is gradually compressed by the wood; but since it is known that in the
growth of the tree much compression of the previously formed wood must
occur, and since this compression is a likely theory by which to account
for the disappearance of the less resisting pith, it is now generally
considered to be one of the causes of this occurrence. As a general rule,
the pith, so long as it exists, is not mingled with other than cellular
structures; but, in certain instances, wooden fibre has been found with
it, and, in others, spiral vessels have been detected.

MEDULLARY SHEATH.--Immediately surrounding the pith of all exogenous
plants, there is a layer of longitudinal tissue, which has received
the name of medullary sheath. This sheath has no special walls, but is
bounded by the pith on the inner, and the wood on the outer side. It is
in this situation that ducts of various kinds and spiral vessels may be
found, and in all cases it conveys the longitudinal structure from the
root, direct to each leaf. The integrity of this structure is therefore
highly necessary to the life of the tree.

MEDULLARY RAYS.--These structures come next in order, and, as has been
previously intimated, belong to the horizontal cellular system of the
stem; they constitute the channel of communication between the bark and
the pith, and are composed of a series of walls of single cells resting
upon the root, and proceeding to the top of the tree, and radiating from
the centre. They lie between the wedge-like blocks of wood, and as they
have a lighter colour than the wood, they are evident on an oblique
section of any stem, and are called the silver grain. Their colour and
number suffice to enable anyone to distinguish various kinds of wood, and
greatly increase their beauty. They cannot, of course, exist before the
wood is formed, and are therefore not met with in very young trees. They
commence to exist with the first deposited layers of wood, and continue
to grow outwardly, or nearest to the bark, so long as the wood continues
to be deposited. In those woods which possess in abundance the silver
grain, another source of ornament exists, viz. a peculiar damask or
dappled effect, somewhat similar to that artificially produced on damask
linens, moreens, silks, and other fabrics, the patterns on which result
from certain masses of the threads on the face of the cloth running
lengthways, and other groups crossways. This effect is observable in a
remarkable degree in the more central planks of oak, especially in Dutch
wainscot.

THE BARK.--As the medullary rays terminate in the bark, on their outer
side, the consideration of that part next follows. It forms the sheath
of the tree, and its more immediate use is that of giving protection to
the wood. If bark did not exist, there would be no formative fluid, and
without formative fluid there could not be any deposit of woody fibre.

WOOD.--We find wood occupying nearly the whole body of the trunk of the
tree, and arranged, as a rule, in a very regular manner. On taking up
any piece of wood, but more particularly the entire section of a stem,
we first notice a series of circles, which increase in diameter and
separate by wider intervals as we approach the bark. In this manner the
trunk is composed of numerous zones enclosed within each other. Again,
in almost all trees, the medullary rays before mentioned may be observed
passing in straight lines from the centre to the circumference; and, as
the circle of the stem at the bark is much larger than any circle near to
the centre, it follows that the medullary rays will be wider apart at the
bark than at the pith. On this view of the subject it may be stated that
the stem is composed of a series of wedge-shaped blocks, which have their
edges meeting at the centre. The combination of these two views gives the
correct idea of the arrangement of the wood, viz. a series of wedges,
each divided into segments of unequal width by circular lines passing
across them. From this description it must not be imagined that these
various portions are detached from each other; for although the medullary
rays and the circular mode of deposition both tend to a less difficult
cleavage of the wood, they yet bind the parts very closely to each other.

The explanation of the occurrence of distinct zones of wood is, that each
zone is the produce of one year, and that in our climate, more so than in
tropical climates, the period of growth of wood ceases for many months
between the seasons, and this induces a distinction in appearance between
the last wood of a former, and the first wood of a succeeding year. This
distinction is maintained throughout each year, and throughout a long
series of years.

The enclosure of zone within zone, is owing to the mode in which the wood
is produced, and the position in which it is deposited. Wood is formed by
the leaves during the growing season, and passes down towards the root
between the bark and the wood of the previous year; and, as the leaves
more or less surround the whole stem, the new layer at length completes
a zone, and perfectly encloses the wood of all former years. This is
the explanation of the term exogenous, which is derived from two words
signifying to grow, outwardly, for the stem increases in thickness by
successive layers on the outer side of the previously formed wood.

The thickness of the zone for the year is rarely equal around the whole
circumference of the stem, and this is due to the lesser abundance
of leaves on the branches of one side than on the other, or to the
prevalence of winds, or some other physical cause, acting in that
direction in opposition to the growing process. It should be observed
that there is not in timber any appearance of a gradual change from
alburnum to perfect wood. On the contrary, in all cases the division is
most decided; one concentric layer being perfect wood, and the next in
succession sap-wood.

The age of trees has been inferred, when a section of the whole stem
could be examined, by counting the number of rings of wood which have
been deposited around the pith. In tropical countries, however, this
method cannot be always relied upon.

Woods are variable in quality according to the nature of the climate, and
of the soil, as also in a considerable degree to the aspect in which they
are situated. Trees grown slowly in open, dry, and exposed situations
are more fine and close in their annual rings, and more substantial
and durable, than those which are grown in close and shady forests, or
rapidly reared in moist or sappy places, the latter being soft and broad
in their rings, and very subject to decay; and their pith is not always
quite in the centre, for the layers are variable also.

The waggon maker takes care to combine toughness and durability by
selecting his wood from trees of second growth, or from trees of first
growth that from infancy have stood alone, or far apart. If the soft wood
trees have stood alone, and are very large (as is often the case with
some of the pines), and most of the branches are near the top, the wood
near the base of the trunk is sometimes found to be _shaky_. This defect
is produced by the action of heavy winds on the top of the tree, which
wrenches or twists the butt, and thus cleaves apart the fibres of the
wood. If the main-top (_couronnement_, of French writers) of a tree dies
while the tree is yet standing, it indicates that water has found its way
into the trunk, and that the tree is in a state of decay.

The fir which grows on very dry marl, forms very narrow yearly rings; if
on rich or damp marl, they are wide; and when on wet soil, they are again
smaller. The common fir on moor soil, has even smaller yearly rings than
if on dry sand or marl. From this it is evident that too wet or too dry a
soil is not suitable for this tree.

The alder and the willow grow best on wet soil, and thrive but poorly
when standing dry.

The weight of wood is of great importance, because its hardness,
resistance, and its heating power, as well as other valuable properties,
are all more or less depending upon it. In the first place, we must
consider that even wood which has been forested very light will become
heavy, when put for some time into water, but in such timbers the sap is
already given to dissolution. If the fibre were the only substance in
the wood, then the specific weight would depend upon the number of pores
contained in its body; the pores are, however, filled with a substance
such as resin, die, &c. Some years since, when the Indian railways
were being formed, the native wood-cutters were so well aware of the
above-mentioned fact, that they used to cut down the soft and inferior
woods in the forests; soak them in water for a certain time; and then
endeavour to pass them to the railway contractors as sound, heavy, and
good railway sleepers, and the latter, not being acquainted with the
Indian woods, were, at first, often deceived.

The hardest, and heaviest woods come from the hotter climates; the only
exception is the pine, which thrives considerably better, and furnishes
heavier timber, when it has grown in colder regions, or upon high
mountains.

Trees grown on northern slopes furnish lighter timber than if grown on
southern or western. The soil has great influence upon the width of the
yearly rings, and from this we are able to come to a conclusion in regard
to the specific weight. In the fir and larch trees the wood is heaviest
when their rings are smallest.

The difference in the strength of timber between the south and the
north side is attributable to the grain being closer on the north side,
as the sap does not rise in the same proportion as upon the south.
In forest-grown wood the difference is almost imperceptible, as the
sun cannot act upon the trunk of the tree; in open-grown timber, the
difference is really perceptible. It is well known that all woods do not
lose strength by being open grown, or, in other words, that the south
side is not always weaker than the north; that theory only applies to
the coniferæ species. In ash it is the opposite, as the south side is
the strongest. In soft-wooded trees, as the acer species, the difference
is not perceptible, as the annual rings, and the intervening cellular
tissues, are so close akin as to render the wood so compact in its grain
that there is no difference in its strength. The coniferæ species, or the
pines, are the only classes of woods that are stronger on the north side
than on the south: it is well known that the difference originates in the
wood being more open in the grain on the south side than on the north.

An influence upon the specific weight is exercised by the resin, and
the die, which are contained in the interior of the wood. On level dry
ground, or deep sandy soil, we find the fir beautifully red inside;
but when we look at it on lias soil, it shows broad yearly rings, and
hardly any colour at all. The larch tree, again, in such soil, develops
itself well with a rich colour. The cause for these appearances must
therefore rest with the chemical condition of the soil, and its effect
upon the individuality of the fir: it is probably the nature of the soil
that causes the difference of character between Honduras and Spanish
mahogany; Honduras being full of black specks, and Spanish of minute
white particles, as if it had been rubbed over with chalk. Oaks generally
furnish good timber when grown slowly in dry ground, whilst those from
wet soil appear comparatively spongy; similar results are obtained with
other trees.

Many persons constantly employed on wood are of opinion that it becomes
harder if it is worked or barked whilst green.

It is not safe to condemn timber, merely because long cracks are visible
on the surface. Such openings are frequently only superficial, and do not
penetrate deeply into the wood: in such cases it is very little weakened
thereby. It is difficult to obtain timber of large scantling without some
defects of this kind, but care should be taken to ascertain if they are
of a serious nature.

Trees arrive at an age when their wood becomes ripe, and then they are
fit for felling; but as upon the proper method and time for doing this,
the prevention of dry rot frequently hinges, a separate chapter is
devoted to this part of the subject.

CHAPTER II.

ON THE GRADUAL RISE AND DEVELOPMENT OF DRY ROT.

The opinion generally received has drawn a line of discrimination between
the decay accompanied by a vegetable spreading on the surface of the
timber, and that which is effected by an animal existing within it,
which decay is frequently denominated the worm in timber; but as each is
equally entitled to the dreaded appellation, they might more justly be
distinguished as the animal and vegetable rot.

The dry rot in timber derives its name from the effect produced, and
not from the cause: it is so called in opposition to the wet rot, which
is properly denominated, as this exists only in damp situations, and is
applied to the decomposition which takes place in timber containing sap,
and exposed to moisture: but although the dry rot is usually generated
in moisture, in some cases it will flourish independent of extraneous
humidity. Dry rot differs from wet rot in this respect, that the former
takes place only when the wood is dead, whereas the latter may begin when
the tree is standing.

Wet rots are composed of porous fibre running from the rot into the
trunk of the tree. This rot is of a brown colour, and has an offensive
smell. The evil is often found with white spots, the latter of watery
substance: when it has yellow flames, it is very dangerous.

A large quantity of the vegetable kingdom consists of plants differing
totally from the flowering plants in general structure, having no
flowers and producing no seed properly so called, but propagating by
means of minute cellular bodies, called _spores_. These highly organized
vegetables are known to botanists as _Cryptogamia_. Fungi are plants in
which the fructifying organs are so minute, that without the aid of a
powerful microscope they cannot be detected. To the naked eye, the fine
dust ejected from the plant is the only token of reproduction; this dust,
however, is not truly seed, for the word seed supposes the existence
of an embryo, and there is no such thing in the reproductive bodies of
fungi. The correct terms are _spores_, when the seeds are not in a case;
_sporidia_ when enclosed in cases. The spores or sporidia are placed
in or upon the receptacle, which is of very various forms and kinds,
but how different soever these may be, it is the essential part of the
fungus, and in many cases constitutes the entire plant. That portion of
the receptacle in which the reproductive bodies are imbedded is called
the _hymenium_: it is either external, as in the Agaric, where it forms
gills; or included, as in the puff-balls. The _pileus_ of fungi is the
entire head of the plant, not a mere head covering.

Some naturalists have insisted upon the spontaneous production of fungi,
while others maintain that they are produced by seed, which is taken
up and supported in the air until a soil proper for its nourishment is
presented, on which being deposited it springs up of various appearances
according to the principle of the seed, and the nature of the recipient.

It is extremely difficult to give a logical definition of what
constitutes a fungus. It is not always easy with a cursory observation
under the microscope, to determine whether some appearances are produced
by fungi, insects, or organic disease; experience is the safest guide,
and until we acquire that we shall occasionally fail.

In the ‘Index Fungorum Britannicorum,’ 2479 species of British fungi are
enumerated: any detailed account of the arrangement of this extensive
family of plants, or of the character of even its principal sections
would be impossible within the limits of this volume; all that can be
attempted will be a general description of the fungi causing dry rot.

If dry rot shows itself in a damp closet or pantry, the inside of
the china or delf lying there will be coated with a mould, or a fine
powder like brick-dust. This excessively fine powder is no other than
unaccountable myriads of the reproductive spores or _seeds_ of the
fungus; they are red in colour, and are produced on the surface of the
fungus in millions. Certain privileged cells on the face of the fungus
are furnished each with four minute points at their apex, each four
bearing a single brick-red, egg-shaped spore; so that the fruit is spread
over the surface of the fungus in groups of fours. To see the form of
these spores the highest powers of the microscope are required, and then
they can only be viewed as transparent objects. If these excessively
minute bodies be allowed to fall on wet flannel, damp blotting-paper, or
wet wood, they immediately germinate and proceed to reproduce the parent
fungus. The red skin of the spores cracks at both ends, and fine mycelial
filaments are sent out: this is the “mould,” spawn, or mycelium from
which the new fungus (under favourable conditions of continued moisture)
appears.

It matters little where we go: everywhere we are surrounded with life.
The air is crowded with birds and insects; the waters are peopled with
innumerable forms, and even the rocks are blackened with countless
mussels and barnacles. If we pluck a flower, in its bosom we see many a
charming insect. If we pick up a fallen leaf, there is probably the trace
of an insect larvæ hidden in its tissue. The drop of dew upon this leaf
will probably contain its animals, visible under the microscope. The
very mould which covers our cheese, our bread, our jam, or our ink, and
disfigures our damp walls, is nothing but a collection of plants.

The starting point of life is a single cell-that is to say a microscopic
sac filled with liquid and granules, and having within it a nucleus,
or smaller sac. From this starting point of a single cell, this is the
course taken: the cell divides itself into two, the two become four, the
four eight, and so on, till a mass of cells is formed.

The researches of Pasteur show that atmospheric dust is filled with
minute germs of various species of animals and plants, ready to develop
as soon as they fall into a congenial locality. He concludes that all
fermentation is caused by the germination of such infinitesimal spores.
That they elude observation does not seem strange, when we consider that
some infusoria are only ⅟240000 of an inch in length.

It is ascertained that fungi produce seed which contains the properties
of germination; and that vegetable corruption is suited to effect it.
When we contemplate the fineness and volatility of the germs, the
hypothesis will not appear unreasonable that they are conveyed by the
rains into the earth, and are absorbed by vegetables; that with the
sap they are disseminated throughout the whole body, and begin to
germinate as soon as the vegetable has proceeded to corruption. Whatever,
therefore, may be the appearance or situation of the fungus producing the
dry rot, or from whatever substance it originates, that substance must be
in a corrupt state.

Fungi result from, or are attendant on, vegetable corruption, assisted
by an adequate proportion of heat and moisture. The sap, or principle
of vegetation, brought into activity, is, according to the ‘Quarterly
Review,’ No. 15, the cause of dry rot, in as far as it is favourable
to the growth of fungi, as it would seem to be when in a state of
fermentation.

Vegetable corruption invariably presupposes fermentation.

Fermentation is a state of vegetable matter, the component parts of which
have acquired sufficient force to produce an intestinal motion, by which
the earthy saline, the oily and aqueous particles therein contained,
exert their several peculiar attractive and repulsive powers, forming new
combinations, which at first change, and at length altogether destroy
the texture of the substance they formerly composed.

There are two things essential towards creating and supporting the
intestinal motion, namely, heat and humidity; for without heat, the air,
which is supposed to be the cohesive principle of all bodies, cannot be
so rarefied as to resume its elasticity; and without humidity there can
be no intestinal motion.

According to Baron Liebig, the decay of wood takes place in the three
following modes:--First, oxygen in the atmosphere combines with the
hydrogen in the fibre, and the oxygen unites with the portion of carbon
of the fibre, and evaporates as carbonic acid: this process is called
decomposition. Second, we have to notice the actual decay of wood which
takes place when it is brought in contact with rotting substances; and
the third process is called putrefaction. This is stated by Liebig to
arise from the inner decomposition of the wood in itself: it loses its
carbon, forms carbonic acid gas, and the fibre, under the influence of
the latter, is changed into white dust.

The fungus occasioning the dry rot is of various appearances, which
differ according to the situation in which it exists. In the earth, it
is fibrous and perfectly white, ramifying in the form of roots; passing
through substances from the external surface, it somewhat differs from
that form; here it separates into innumerable small branches.

Mr. McWilliam observes, “If the fungi proceed from the slime in the
fissures of the earth, they are generally very ramous, having round
fibres shooting in every direction. If they arise from the roots of
trees, their first appearance is something like hoar frost; but they soon
assume the mushroom shape.”

Hence it appears that we frequently build on spots of ground which
contain the fundamental principle of the disease, and thus we are
sometimes foiled in our endeavours to destroy the fungus by the admission
of air. In this case the disease may be encouraged by the application of
air as a remedy. When workmen are employed in buildings which contain dry
rot, and when they are working on ground which contains the symptoms of
this disease, their health is often affected. A London builder informs
us, that a few years since, while building some houses at Hampstead
his men were never well: he afterwards ascertained that the ground was
affected with rot, and that within one year after the house was erected,
all the basement floor was in a state of premature decay. Sir Robert
Smirke, architect, remarked in 1835, that he had noticed “there are
certain situations in which dry rot prevails remarkably.”

The fungus protruded in a very damp situation is fibrous, of moderate
thickness, feels fleshy. From the spot whence it arises it extends
equally around, wholly covering the area of a circle. This form would
possibly continue in whatever situation it might vegetate, if the air had
no motion, and every part of the substance on which it grew were equally
supplied with a matter proper to encourage the expansion. The surface of
this fungus is pursed, and of various colours, the centre is of a dusky
brown, mixed with green, graduated into a red, which degenerates into
yellow, and terminates in white.

One of the most formidable of the tribe of fungi is the _Merulius
lachrymans_ (often called _the_ Dry Rot) of which the following
description is given by Dr. Greville: “Whole plant generally resupinate,
soft, tender, at first very light, cottony, and white. When the veins
appear, they are of a fine yellow, orange, or reddish brown, forming
irregular folds, most frequently so arranged as to have the appearance
of pores, but never anything like tubes, _and distilling, when perfect,
drops of water_.” Hence the term _lachrymans_, from _lacrymo_, Lat., I
weep: the _Merulius lachrymans_ is often dripping with moisture, as if
weeping in regret for the havoc it has made. In the genus _Merulius_,
the texture is soft and waxy, and the hymenium is disposed in porous or
wavy toothed folds. Berkeley, in his ‘Fungology,’ gives the following
description, which is similar to Dr. Greville’s: “Large, fleshy but
spongy, moist, ferruginous yellow, arachnoid and velvety beneath;
margin tomentose, white; folds ample, porous, and gyroso-dentate.” The
_Merulius_ is found in cellars and hollow trees, sometimes several feet
in width, and is the main cause of dry rot.

Another formidable fungi, which attacks oak in ships, is the _Polyporus
hybridus_ (the dry rot of our oak-built vessels). It is thus described by
Berkeley: “White, mycelium thick, forming a dense membrane, or creeping
branched strings, hymenium breaking up into areæ, pores long, slender,
minute.”

From the slow progress dry rot makes in damp situations, it appears
that excessive damps are inimical to the fungus, for its growth is more
rapid in proportion as the situation is less damp, until arrived at that
certain degree of moisture which is suited both to its production and
vegetation. When further extended to dry situations, its effects are
considerably more destructive to the timber on which it subsists: here
it is very fibrous, and in part covered with a light brown membrane,
perfectly soft and smooth. It is often of much greater magnitude,
projecting from the timber in a white spongeous excrescence, on the
surfaces of which a profuse humidity is frequently observed: at other
times, it consists only of a fibrous and thin-coated web irregularly on
the surface of the wood. Excrescences of a fungiform appearance are often
protruded amidst those already described, and are evidences of a very
corrupt matter peculiar to the spots whence they spring. According to the
situation and matter in which they are produced, they are dry and tough,
or wet, soft, and fleshy, sometimes arising in several fungiforms, each
above the other, without any distinction of stem; and when the matter
is differently corrupted, it not unfrequently generates the small acrid
mushroom.

Mr. McWilliam observes, “The fungi arising from oak timbers are generally
in clusters of from three to ten or twelve; while those from fir timber
are mostly in single plants: and these will continue to succeed each
other until the wood is quite exhausted.”

Damp is not only a cause of decay, but is essential to it; while, on the
other hand, absolute wet, especially at a low temperature, prevents it.
In ships this has been particularly remarked, for that part of the hold
of a ship which is constantly washed by the bilge-water is never affected
with dry rot. Neither is that side of the planking of a ship’s bottom
which is next the water found in a state of decay, even when the inside
is quite rotten, unless the rot has penetrated quite through the inside.

It matters little whether wet is applied to timber before or after
the erection of a building. Timber cannot resist the effect of what
must arise in either case; viz. heat and moisture, producing putrid
fermentation; for instance, in basement stories with damp under them,
dry timber is but little better than wet, for if it is dry it will soon
be wet; decay will only be delayed so long as the timbers are absorbing
sufficient moisture, therefore every situation that admits moisture is
the destruction of timber.

In a constancy and equality of temperature timber will endure for ages.
Sir Christopher Wren, in his letter to the Bishop of Rochester, inserted
in Wadman’s ‘History of Westminster Abbey,’ notices “That Venice and
Amsterdam being both founded on wooden piles immersed in water, would
fall if the constancy of the situation of those piles in the same element
and temperature did not prevent the timber from rotting.” Nothing is more
destructive to woodwork than _partial leaks_, for if it be kept _always
wet_ or _always dry_, its duration is of long continuance. It is recorded
that a pile was drawn up sound from a bridge on the Danube, that parted
the Austrian and Turkish dominions, which had been under water 1500 years.

The writer of an article on the decay of wood, in the ‘Encyclopædia
Britannica,’ 1855, observes, “If a post of wood be driven into the
ground, the decay will commence at the surface of the ground; if driven
into the earth through water, the decay will commence at the surface of
the water; if used as a beam let into a damp wall, rot will commence just
where the wood enters the wall.”

Humboldt observes in his ‘Cosmos,’ with reference to damp and damp rooms,
that anyone can ascertain whether a room is damp or not, by placing a
weighed quantity of fresh lime in an open vessel in the room, and leaving
it there for twenty-four hours, carefully closing the windows and doors.
At the end of the twenty-four hours the lime should be reweighed, and if
the increase exceeds one per cent. of the original weight, it is not safe
to live in the room.

Decay of timber will arise from the effects of continued dryness or
continued wetness, under certain conditions; or it may also arise from
the effect of alternate dryness and moisture, or continued moisture with
heat.

At one time dry rot appears to have made great havoc amongst the wooden
ships of the British Navy. In the Memoirs of Pepys, who was Secretary to
the Admiralty during the reigns of Charles II. and James II., reference
is made to a Commission which was appointed to inquire into the state of
the navy, and from which it appears that thirty ships, called new ships,
“for want of proper care and attention, had toadstools growing in their
holds as big as one’s fists, and were in so complete a state of decay,
that some of the planks had dropped from their sides.”

In the ‘European Magazine’ for December, 1811, it is stated that, “about
1798, there was, at Woolwich, a ship in so bad a state that the deck
sunk with a man’s weight, and the orange and brown coloured fungi were
hanging, in the shape of inverted cones, from deck to deck.”

Mr. William Chapman, in his ‘Preservation of Timber from Premature
Decay,’ &c., gives several instances of the rapid decay of the ships
of the Royal Navy, about the commencement of the present century. He
mentions three ships of 74 guns each, decayed in five years; three of
74 guns each, decayed in seven years; and one of 100 guns, decayed in
six years. Mr. Pering, also, in his ‘Brief Enquiry into the Causes of
Premature Decay,’ &c., says that ships of war are useless in five or
six years; and he estimates the average duration to be eight years, and
that the cost of the hull alone of a three-decker was nearly 100,000_l._
Mr. Pering was formerly at the dockyard, Plymouth, and therefore a good
authority, if he availed himself of the opportunities of studying the
subject. He has stated that he has seen fungi growing so strong betwixt
the timbers in a man-of-war, as to force a plank from the ship’s side
half an inch.

No doubt a great deal of this decay was attributable to the use of
unseasoned timber, and defective ventilation; but there is too much
reason to believe that it was principally owing to the introduction
of an inferior species of oak (_Quercus sessiliflora_) into the naval
dockyards, where, we imagine, the distinction was not even suspected. The
true old English oak (_Quercus robur_) affords a close-grained, firm,
solid timber, rarely subject to rot; the other is more loose and sappy,
very liable to rot, and not half so durable.

One cause of the decay of wood in ships is the use of wooden treenails.
A treenail is a piece of cleft wood (made round), from 1 foot to 3
feet 6 inches in length and 1½ inch in diameter. As the treenails are
also made to drive easy, they never fill the holes they are driven
into; consequently, if ever it admits water at the outer end, which,
from shrinking, it is liable to do, that water immediately gets into
the middle of the plank, and thereby forms a natural vehicle for the
conveyance of water. The treenail is also the second thing which decays
in a ship, the first, generally, being the oakum. Should any part of
the plank or timbers of a ship be in an incipient state of decay, and a
treenail come in contact with it, the decay immediately increases, while
every treenail shares the same fate, and the natural consequence is, the
ship is soon left without a fastening. Treenails in a warm country are
sure to shrink and admit water.

Mr. Fincham, formerly Principal Builder in Her Majesty’s dockyard,
Chatham, considers that the destruction of timber by the decay commonly
known as dry rot, cannot occur unless air, (?) moisture, and heat are
all present, and that the entire exclusion of any of the three stays the
mischief. By way of experiment, he bored a hole in one of the timbers of
an old ship built of oak, whose wood was at the time perfectly sound;
the admission of air, the third element, to the central part of the wood
(the two others being to a certain degree present) caused the hole to be
filled up in the course of twenty-four hours with mouldiness, which very
speedily became so compact as to admit of being withdrawn like a stick.

The confinement of timber under most circumstances is attended with the
worst consequences, yet a partial ventilation tends to fan the flame of
decay.

The admission of air has long been considered the only means of
destroying the fungus, but as it has frequently proved ineffectual, it
must not be always taken as a certain remedy. If dry air be properly
admitted, in a quantity adequate to absorb the moisture, it will
necessarily exhaust and destroy the fungus; but care should be taken lest
the air should be conveyed into other parts of the building, for, after
disengaging itself from the fungus over which it has passed, it carries
with it innumerable seeds of the disease, and destroys everything which
offers a bar to its progress. Air, in passing through damps, will partake
of their humidity; it therefore soon becomes inadequate to the task for
which it is designed. Owing to this circumstance, air has been frequently
admitted into the affected parts of a building without any ultimate
success; too often, instead of injuring the fungus, it has considerably
assisted its vegetation, and infected with the disease other parts of the
building, which would otherwise probably have remained without injury.
The timber, which is in a state of decomposition by an intestinal decay,
is little affected by the application of air, as this cannot penetrate
the surrounding spongeous rottenness which generally forms the exterior
of such timber, and protects the action which the humid particles have
acquired in the exterior: as the extent and progress of the disease
is therefore necessarily concealed, it is difficult to ascertain
correctly the effect produced by the admission of dry air. Under these
circumstances of necessity and danger, it will require considerable
skill to effect the purpose without increasing the disease, and, as each
case has its own peculiar characteristics, it is necessary before one
attempts to admit air as a remedy, to previously estimate the destructive
consequences which may result from so doing, and ascertain whether it
will be injurious or beneficial to the building. The joists of the houses
built by our ancestors last almost for ever, because they are in contact
with an air which is continually changing. Now, on the contrary, we
foolishly enclose them between a ceiling of plaster (always very damp to
begin with) and a floor; they frequently decay, and then cause the most
serious disasters, of which it is impossible to be forewarned.

Damp, combined with warmth, is as a destroying agent, still more active
than simple damp alone--the heat being understood as insufficient to
carry off the moisture by evaporation; and the higher the temperature
with a corresponding degree of moisture, the more rapid the decay. If
the temperature to which wood is exposed, whilst any sap remains in
it, is too elevated, the vegetable fluids ferment; the tenacity is
diminished, and when the action is carried to its full extent, the wood
quickly becomes affected by the dry rot. Exposure to the atmosphere in
positions where rain can lodge in quantity, contact with the ground, and
application in damp situations deprived of air, will render wood liable
to the wet rot; and however well seasoned it may have been previously
to being brought within the influence of any of these causes, it will
infallibly suffer. Air should therefore have free access to the wood in
every direction:

… “for without in the wall of the house he made narrowed rests
round about, that the beams should not be fastened in the walls
of the house.”--1 Kings vi. 6.

Rondelet says, “The woodwork of the church of St. Paul, outside the city
walls, which was destroyed by fire in 1823, was erected as far back as
the fifth century.” Although the atmosphere surrounding the framework
was often at once warm and damp, yet it was never stagnant. It should be
remembered that 500 people in a church during two hours give off fifteen
gallons of water into the air, which, if not carried away, saturates
everything in the building after it has been breathed over and over
again in conjunction with the impurities it contains collected from each
individual.

Fever, scrofula, and consumption arise in many instances from defective
ventilation.

The signs of decay in timber are, as has been stated, fungi. Some of them
now and then are microscopic, and owe their existence to the sporules
deposited on the surface; while fermentation, generated by prolonged
contact with warm, damp, and stagnant air, is as a soil where seeds sow
and nourish themselves.

Mr. McWilliam, in his work on dry rot, states that if the temperature
be very low or very high, the effects are the same with respect to the
growth of fungi. At 80° dry rot will proceed rapidly, at 90° its progress
is more slow; at 100° it is slower still, and from 110° to 120° it will
in general be arrested. It will proceed fast at 50°; it may be generated
at 40°; its progress will be slow at 36°; and is arrested at 32°, yet it
will return if the temperature is raised to 50°.

Dry rot externally first makes its appearance as a mildew, or rather
a delicate white vegetation, that looks like such. The next step is a
collecting together of the fibres of the vegetation into a more decided
form, somewhat like hoar frost; after which it speedily assumes the
leathery, compact character of the fungus, forming into leaves, spreading
rapidly in all directions, and over all materials, and frequently
ascending the walls to a considerable height, the colour variable--white,
greyish white, and violet, light or decided brown, &c.

In the section of a piece of wood attacked by dry rot a microscope
reveals minute white threads spreading and ramifying throughout its
substance; these interlace and become matted together into a white
cottony texture, resembling lint, which effuses itself over the surface
of the timber; then in the centre of each considerable mass a gelatinous
substance forms, which becomes gradually of a yellow, tawny hue, and a
wrinkled, sinuated porous consistence, shedding a red powder (the spores)
upon a white down; this is the resupinate pileus, the hymenium being
upwards, of _Merulius lachrymans_, in its perfect and matured state. Long
before it attains to this, the whole interior of the wood on which it
is situated has perished; the sap vessels being gradually filled by the
cottony filaments of the fungus; no sooner do these appear externally
than examination proves that the apparently solid beam may be crumbled
to dust between the fingers; tenacity and weight are annihilated.

Dr. Haller says that seven parts in eight of a fungus in full vegetation
are found by analysis to be completely aqueous.

The strength of fungi is proportionate to the strength of the timber the
cohesive powers and nutritive juices of which they absorb; and according
to the food they receive so they are varied and modified in different
ways, and are not always alike. Different stages of corruption produce
food of different qualities, and hence many of the different appearances
of fungi. One takes the process of corruption up where another leaves it
off, and carries it forward and farther forward to positive putrefaction.

The forms which fungi assume are extremely diversified; in some instances
we have a distinct stem supporting a cap, and looking somewhat like a
parasol; in others the stem is entirely absent, and the cap is attached
either by its margin, and is said to be _dimidiate_, or by its back,
or that which is more commonly its upper surface, when it is called
_resupinate_. In some species the form is that of a cup, in others of
a goblet, a saucer, an ear, a bird’s nest, a horn, a bunch of coral, a
ball, a button, a rosette, a lump of jelly, or a piece of velvet.

Decomposition takes place without fungus where the timber and the
situation are always moist, as in a close-boarded kitchen floor, where
it is always dry, or very nearly so, and where it is alternately wet
and dry, cold and hot. When the decomposition is affected with very
little moisture, and no fungus, the admission of air will generally
prevent further contamination; but where there is abundance of moisture,
rottenness, and fungus, a small quantity of air will hasten the
destruction of the building.

In timber which has been only superficially seasoned this disease is
produced internally, and has been known to convert the entire substance
of a beam, excepting only the external inch or two of thickness to
which the seasoning had penetrated, into a fine, white, and threadlike
vegetation, uniting in a thick fungous coat at the ends, the semblance
being that of a perfectly sound beam. In this internal rot a spongy
fungous substance is formed between the fibres. This has often been
observed in large girders of yellow fir, which have appeared sound on
the outside, but by removing some of the binding joists have been found
completely rotten at the heart. An instance of this kind occurred at
Kenwood (the seat of the Earl of Mansfield) in 1815. Major Jones, R.E.,
states that on one occasion he was called upon to report on the state of
a building in Malta; that the timbers had every external appearance of
being sound, but on being bored with an auger they were found internally
in a total state of decay. It is on this account that the practice of
sawing and bolting beams is recommended, for when timber is large enough
to be laid open in the centre this part is laid open to season; so that
when a tree is large enough to be cut through to make two or more beams,
decomposition is impeded.

The first symptoms of rottenness in timber are swelling, discoloration,
and mouldiness, accompanied with a musty smell; in its greater advance
the fibres are found to shrink lengthways and break, presenting many deep
fissures across the wood; the fibres crumble readily to a fine snuff-like
powder, but retain, when undisturbed, much of their natural appearance.

In whatever way boughs are removed from trees, the effect of their
removal is, however, very frequently to produce a rotting of the inner
wood, which indicates itself externally by a sudden abnormal swelling of
the trunk a little above the root; sometimes the trunk becomes hollow at
the part affected, and this particular description of rot will almost
invariably be found to exist in those trees whose roots are much exposed.
The rot itself is either of a red, black, or white colour in the timber
when felled, and when either of the two last-named colours prevail, it
will be found that the decay does not extend very far into the tree;
but if, on the contrary, the colour of the parts most visibly affected
should be decidedly red, the wood should be rejected for any building
purposes. Sometimes small brown spots, indicative of a commencement of
decay, may be observed near the butt or root end of trees, and though
they do not appear to be connected with any serious immediate danger to
the durability of the wood, it is advisable to employ the material so
affected only in positions where it would not be confined in anything
like a close, damp atmosphere.

Great hesitation may be admitted as to the use of timber which presents
large bands of what are supposed to be indefinitely-marked annual
growth, because the existence of zones of wood so affected may be
considered to indicate that the tree was not in a healthy state when they
were formed, and that the wood then secreted lacked some of the elements
required for its durability, upon being subsequently exposed to the
ordinary causes of decay.

In many cases when timber trees are cut down and converted for use, it
is found that at the junction of some of the minor branches with the
main stem, the roots, as it were, of the branches traverse the surface
wood in the form of knots, and that they often assume a commencement of
decay, which in the course of time will extend to the wood around them.
This decay seems to have arisen in the majority of cases from the sudden
disruption of the branch close to its roots, with an irregular fracture,
and with such depressions below the surface as to allow the sap to
accumulate, or atmospheric moisture to lodge in them. A decomposition of
the sap takes place--in fact, a wound is made in the tree-and what are
called “druxy knots” are thus formed, which have a contagious action on
the healthy wood near them.

There is this particular danger about the dry rot; viz. that the germs
of the fungi producing it are carried easily, and in all directions, in
a building wherein it once displays itself, without necessity for actual
contact between the affected or the sound wood; whereas the communication
of the disease resulting from the putrefactive fermentation, or the wet
rot, only takes place by actual contact.

[Illustration: _Timber Beams,--rotten at the heart._]

Before dry rot has time to destroy the principal timbers in a building,
it penetrates behind the skirtings, dadoes, and wainscotings, drawing
in the edges of the boards, and splitting them both horizontally and
vertically. When the fungus is taken off, they exhibit an appearance
similar both in back and front to wood which has been charred; a light
pressure with the hand will break them asunder, even though affected with
the rot but a short time; and in taking down the wainscot, the fibrous
and thin-coated fungus will generally be seen closely attached to the
decayed wood. In timber of moderate length the fungus becomes larger and
more destructive, in consequence of the matter congenial to its growth
affording a more plentiful supply.

It is a great characteristic of fungi in general that they are very
rapid in growth, and rapid in decay. In a night a puff-ball will grow
prodigiously, and in the same short period a mass of paste may be covered
with mould. In a few hours a gelatinous mass of _Reticularia_ will pass
into a bladder of dust, or a _Coprinus_ will be dripping into decay. Many
instances have been recorded of the rapidity of growth in fungi; it may
also be accepted as an axiom that they are in many instances equally as
rapid in decay.

In considering the liability of any particular description of foreign
timber to take the dry rot, attention must be paid to the circumstances
under which it is imported. Sometimes the timber is a long while coming
here, whilst at other times it is imported in a very short period. The
length of time consumed in the voyage has a great deal to do with its
likelihood of taking the rot: it may have a very favourable passage, or
a very wet one, and the ship is frequently, in some degree, affected
with the disease. It perhaps begins in the ship, and it may often be
seen between the timber or deals, when it will impregnate the wood to a
great depth. Whether it is inherent in the timber or not, of this we may
be certain, that where there is a fetid atmosphere it is sure to grow.
Canadian yellow wood pine timber is more subject to rot than Baltic or
Canadian red wood timber, although the latter will sometimes decay in
four or five years. Turpentine is a preventive against dry rot, and
Canadian timber is sometimes largely impregnated with it, especially the
red wood timber; the yellow wood is very subject to dry rot. Very few
cargoes of timber in the log arrive from Canada in which in one part or
other of nearly every log you will not see a beginning of the vegetation
of the rot. Sometimes it will show itself only by a few reddish,
discoloured spots, which, when scratched by the finger nail to the extent
of each spot, it will be seen that the texture of the timber to some
little depth is destroyed, and will be reduced to powder; and on these
spots a white fibre may generally be seen growing. If the timber has been
shipped in a dry condition, and the voyage has been a short one, there
may be a few logs without a spot; but generally speaking very few cargoes
arrive from Canada in which there are many logs of timber not affected.
But if the cargo has been shipped in a wet condition, and the voyage has
been a long one, then a white fibre will be seen growing over nearly
every part of the surface of every log; and in cargoes that have been so
shipped, all the logs of yellow pine, red pine, and of oak, are generally
more or less affected on the surface.

Nearly every deal of yellow pine that has been shipped in Canada in a
wet state, when it arrives here is also covered over with a network of
little white fibres, which are the dry rot in its incipient state. There
is no cargo, even that which is shipped in tolerably dry condition, in
which, upon its arriving here, may not be found some deals, with the
fungus beginning to vegetate on their surface. If they are deals that
have been floated down the rivers of America or Canada, and shipped in a
wet state, on their arrival here they are so covered with this network
of the fungus, that force is often necessary to separate one deal from
another, so strongly does the fungus occasion them to adhere. They grow
together again, as it were, after quitting the ship, while lying in the
barges, before being landed. Accordingly, if a cargo has arrived in a wet
condition, or late in the year, or if the rain falls on the deals before
they are landed, and they are then piled in the way in which Norwegian
and Swedish deals are piled, that is, flatways, in six months time, or
even less, the whole pile of deals become deeply affected with rot; so
that, whenever a flat surface of one deal is upon the flat surface of
another, the rot penetrates to the depth of ⅛ of an inch. Its progress
is then arrested by repiling the deals during very dry weather, and by
sweeping the surface of each deal before it is repiled: but the best way
is to pile the deals in the first instance upon their edges; by which
means the air circulates freely around them, the growth of the fungus
is arrested, and the necessity of repiling them prevented. If the ship
is built of good, sound, and well-seasoned oak, the rot would perhaps
not affect it, but in order to prevent its doing so, the precaution is
usually taken to scrape the surface as soon as the hold is clear of the
cargo of timber. Were the cargo not cleared, and the hold not ventilated,
a ship that was permanently exposed to this fungus would, no doubt, be
affected. It is easy, however, to prevent its extending by washing the
hold with any desiccating solution.

Anyone who wishes to know how timber is occasionally shipped to this
country should read the report of a trial, in the ‘Times,’ 22nd Feb.,
1875 (Harrison _v._ Willis), relative to a cargo of pitch pine shipped
from Sapelo, in the Isthmus of Darien, for Liverpool. This cargo,
however, never arrived at Liverpool: it was lost at sea.

The motto of the Worshipful Company of Shipwrights is, “Within the ark,
safe for ever.” We suggest it should be altered to, “Within the ark
_which is free from dry rot_, safe for ever.”

There are two descriptions of European deals very liable to take the dry
rot; viz. yellow Petersburgh deals, and yellow and white battens, from
Dram, in Norway. When Dram battens, which have been lying a long time in
bond in this country, have not been repiled in time, they have been found
as much affected with the dry rot as many Canadian deals; though this has
not happened in so short a time as has been sufficient to rot Canadian
deals. The fungus growing on the Petersburgh deals and Dram battens
has all the characteristics and effects of dry rot as exhibited in the
Canadian deals, the detection of dry rot being in most cases the same.

It should be remembered that white deal absorbs more water than yellow;
and yellow more water than red; and the quantity of water absorbed by
the white accounts for its more rapid decay in external situations; as
the greater the quantity of water absorbed the quicker is the timber
destroyed. Mr. John Lingard, in his work on timber (1842), states that he
has proved that 4½ oz. of water can be driven off from a small piece of
fir, weighing only 10 oz. when wet, which is nearly half. This timber was
on a saw-pit, and going to be put into a building.

The most general, and the most fatal cause of decay, viz. the wet rot,
has attracted less attention than the more startling, but less common
evils, the dry rot, and the destruction by insects.

Sir Thomas Deane, in 1849, related before the Institution of Civil
Engineers of Ireland, an extraordinary instance of the rapid decay of
timber from rot, which occurred in the church of the Holy Trinity at Cork.

On opening the floors under the pews, a most extraordinary appearance
presented itself. There were flat fungi of immense size and thickness,
some so large as almost to occupy a space equal to the size of a pew,
and from 1 to 3 inches thick. In other places fungi appeared, growing
with the ordinary dry rot, some of an unusual shape, in form like a
convolvulus, with stems of from a quarter to half an inch in diameter.
When first exposed, the whole was of a beautiful buff colour, and emitted
the usual smell of the dry-rot fungus.

During a great part of the time occupied in the repairs of the church,
the weather was very rainy. The arches of the vaults having been turned
before the roof was slated, the rain water saturated the partly decayed
oak beams. The flooring and joists, composed of fresh timber, were laid
on the vaulting before it was dry, coming in contact at the same time
with the old oak timber, which was abundantly supplied with the seeds of
decay, stimulated by moisture, the bad atmosphere of an ill-contrived
burial-place, and afterwards by heat from the stoves constantly in use.
All these circumstances account satisfactorily for the extraordinary and
rapid growth of the fungi.

Many instances might be mentioned of English oak being affected with
dry rot, under particular circumstances. There was a great deal at the
Duke of Devonshire’s, at Chiswick, about 60 years ago. Needy builders,
who work for contract, sometimes use American oak, and call it wainscot:
it is a bad substitute for wainscot, being very liable to warp and to
be affected with dry rot. “I know of one public building,” observed the
late Mr. Henry Warburton, M.P., “in which it has been introduced, and, I
suppose, paid for under that name.”

Another serious instance of the decay of timber from rot occurred some
time since in Old St. Pancras Church, London. When the dry rot made its
appearance, it spread with amazing rapidity. Sometimes in the course of a
night, a fungus of about the consistence of newly-fallen snow, and of a
yellowish-white unwholesome colour, would be found to have spread over a
considerable surface. The fungus was without shape, but in some cases it
rose to a height of 2, 3, or 4 inches above the planks or other surfaces
on which it grew. It could be cut with a knife, leaving a clear edge on
each side, and there did not seem to be any covering or membrane over
the outer or under surface. The smell of those matters was unpleasant,
and seemed like the concentration of the smell which had pervaded the
church for so long a time before; and, in a short time, beams, planks of
flooring, railings, &c., were reduced to rottenness: the colour changed,
and a heavy dark-brown dust fell, and represented the once solid timber.
On making an examination with a view of discovering the cause of the
attack, it was found that in the graveyard, near the church, there were
graves, and several vaults: there were also vaults in the inside of the
church. Most of them were filled, or nearly so, with water, which had run
from the overcrowded graves.

In the interior there were water-logged vaults, and the walls were
saturated with damp. It was also seen that from want of proper spouts
and drains, near the outer walls, the drip from the large pent roof had
fallen into the foundations. In this situation, when the window frames
were properly arranged, a drain dug round and from parts of the church,
and other alterations, which should long before have been made, were
completed, the dry rot vanished, and no more complaints of the foulness
of the air have since been heard.

We could quote many cases of rot which have been caused from the want of
proper drains and spouts. Architects should remember that the feet of
Gothic collar roofs have to bear the whole weight of the roof, and unless
well seasoned, and carefully protected from damp, leaks, &c., premature
decay and dry rot will be sure to occur. It is surprising what injury
leaks from gutters will sometimes do. In 1851, Professor T. L. Donaldson
stated that “a brestsummer of American timber was used some time since
at a house in London: after an expiration of three years cracks began to
appear in the front wall. A friend of mine, an architect, was called in
to find out the cause; and after examining different parts of the house,
was almost giving up his search in despair, when he thought he would have
the shop cornice removed and look at the brestsummer. He then discovered
that some water had been admitted by accident, and penetrating the
brestsummer, had caused it to rot, and crack the wall.”

Dry rot was found in the great dome of the Bank of England, London, as
originally built by Sir Robert Taylor: it also existed in the Society of
Arts building, in the Adelphi, London. It was also found in the domes of
the Panthéon, and Halle-au-Blé, Paris; but we hope there is no dry rot in
the dome of St. Paul’s Cathedral, London, which is constructed entirely
of timber, covered externally with lead.

The decayed state of a barn floor attacked by rot is thus described by
Mr. B. Johnson: “An oak barn floor which had been laid twelve years began
to shake upon the joists, and on examination was found to be quite rotten
in various parts. The planks, 2½ inches in thickness, were nearly eaten
through, except the outsides, which were glossy, and apparently without
blemish. The rotten wood was partly in the state of an impalpable powder,
of a snuff colour; other parts were black, and the rest clearly fungus.
No earth was near the wood.” This oak was probably of the _Quercus
sessiliflora_ species; and there was no ventilation to the floor.

Mr. John Armstrong, carpenter, employed for many years at Windsor Castle,
observed: “I was employed a few years back at a house where I found a
floor rotten. We took it up; it was yellow pine; it was laid in the
damp, but on sleepers, and the sleepers were not rotten: they were of a
different description of wood.” Probably the sleepers were of Baltic red
wood.

Dr. Carpenter relates an instance of the expansive power resulting
from the rapid growth of the soft cellular tissue of fungi. About the
commencement of this century the town of Basingstoke was paved; and not
many months afterwards the pavement was observed to exhibit an unevenness
which could not easily be accounted for. In a short time after, the
mystery was explained, for some of the heaviest stones were completely
lifted out of their beds by the growth of large toadstools beneath them.
One of these stones measured 22 inches by 21 inches, and weighed 83 lb.,
and the resistance afforded by the mortar which held it in its place
would probably be even a greater obstacle than the weight. A similar
incident came under the notice of Mr. M. C. Cooke (the author of ‘British
Fungi’), of a large kitchen hearthstone which was forced up from its bed
by an under-growing fungus, and had to be relaid two or three times,
until at last it reposed in peace, the old bed having been removed
to the depth of 6 inches, and a new foundation laid. A circumstance
recorded by Sir Joseph Banks is still more extraordinary, of a cask of
wine which, having been confined for three years in a cellar, was, at
the termination of that period, found to have leaked from the cask, and
vegetated in the form of immense fungi, which had filled the cellar, and
borne upwards the empty wine cask.

Timber decay in contact with stone is a subject deserving consideration.
This decay is entirely obviated by inserting the wood in an iron shoe,
or by placing a thin piece of iron between the wood and the stone. It is
said that a hard crust is formed on the timber in contact with the iron,
which seems effectually to preserve it; it is, of course, necessary that
a free circulation of air round the ends of the timber be provided. The
most notable instance of timber decay in contact with stone with which we
are acquainted occurred at the coronation of George IV. Westminster Hall
was then fitted up, and they began by laying sleepers of yellow pine. The
coronation was suspended for twelve months, and when the sleepers were
taken up from the floor of Westminster Hall, they were in a rotten state.

Timber in contact with brickwork is in Suffolk and in some parts of
England covered with sheet lead to preserve it from the effects of the
damp mortar. Fungi will arise in mortar, if made with road-drift, and
water from stagnant ponds, &c., and it may be traced through the mortar
joints, and will thus appear on both sides of a wall. Mortar composed of
unwashed sand will generate fungi; sea sand, even if washed, should never
be used. It is considered that the system of grouting contributes to the
early decay of timber; wood bond timber for walls has been consequently
replaced by hoop iron bond. In Manchester wood bond is frequently used,
and is said to answer well, but the high temperature of the buildings may
be a preventive against the decay of timber, as the walls are soon dried.
The practice is a bad one.

When timber used as posts inserted in the ground is placed in the
inverted position to that in which it stood when growing, it is said
to be very much more durable than if placed in its natural or growing
position. This is easily accounted for in the valves of the sap vessels
of the growing timber opening upwards; but when that position is
inverted, the valves of the sap vessels become reversed in their action;
and, therefore, when timber is used as posts inserted in the ground, the
valves being so reversed prevent the ascent of moisture from the soil in
the wood. Mr. W. Howe relates an experiment made to test the comparative
durability of posts set as they grew. He says, “Sixteen years ago I set
six pairs of bar posts all split out of the butt end of the same white
oak log. One pair I set butts down; another pair, one butt down, the
other top down; the others top down. Four years ago those set butt down
were all rotted off, and had to be replaced by new ones. This summer I
had occasion to reset those that were set top down: I found them all
sound enough to reset. My experiments have convinced me that the best
way is to set them tops down.” Other instances might be given in favour
of placing posts in an inverted position in the ground. Posts will
sometimes decay, for the following reason: The ends are often sawn off
with a coarse implement and left spongy, with the longitudinal fibres
shaken or broken a considerable way within the extremity of the wood. In
this state the ends of the posts must be apt to absorb from the ground
the moisture, which, being retained, and speedily pervading the whole
internal surface, _especially if painted_, appears to cause decay.

With respect to the preservation of wooden fences, Mr. Cruikshank, of
Marcassie, gives in detail various experiments from which it appears
that--1st. When larch or pine wood is to be exposed to the weather, or
to be put in the ground, no bark should be left on. 2nd. When posts are
to be put in the ground, no earth should be put round them, but stones.
3rd. When a wooden fence is to be put up, a No. 4 or No. 5 wire should be
stretched in place of, or alongside the upper rail.

Mr. G. S. Hartig, in the ‘Revue Horticole,’ gives the results of
experiments made with great care and patience, upon woods buried
in the earth. Pieces of wood of various kinds 3⅛th inches square,
were buried about one inch below the surface of the ground, and they
decayed in the following order: the lime, American birch, alder,
and the trembling-leaved poplar, in three years; the common willow,
horse-chestnut, and plane, in four years; the maple, red beech, and
common birch, in five years; the elm, ash, hornbeam, and Lombardy
poplar, in six years; the oak, Scotch fir, Weymouth pine, and silver
fir, were only decayed to the depth of half an inch in seven years;
the larch, common juniper, red cedar, and arbor vitæ, at the end of
the last-mentioned period remained uninjured. The duration of their
respective woods greatly depends on their age and quality; specimens from
young trees decaying much quicker than those from sound old trees; and,
when well seasoned, they, of course, last much longer than when buried in
an unseasoned state. In experiments with the woods cut into thin boards,
decay proceeded in the following order: the plane, horse-chestnut,
poplar, American birch, red beech, hornbeam, alder, ash, maple, silver
fir, Scotch fir, elm, Weymouth pine, larch, locust oak.

Before quitting the subject of decay of timber when buried in the earth,
it will not be out of place to allude to the decay of railway sleepers,
taking for example those in India: English and American sleepers will be
dealt with more in detail hereafter.

Dr. Cleghorn, Conservator of Forests, Madras Presidency, India, considers
the decay of sleepers to arise in a great measure from the inferior
description of wood used. Mr. Bryce McMaster, Resident Engineer,
Salem, considers that the native wood sleepers in India have hitherto
been found for the most part to fail on the Madras Railway, between
30 and 40 per cent. requiring to be renewed annually. Mr. McMaster
undertook an investigation with a view of ascertaining the causes of
this deterioration, and whether those causes could be overcome so as to
render available the vast resources of India. Thirteen hundred sleepers
of sixteen different woods were submitted to careful examination and
scrutiny twice at an interval of one year. The sleepers were variously
placed, both on embankments and in cuttings; in some cases they were
entirely covered with ballast to a depth of 4 inches; while in others
they were as much as possible uncovered, and completely so from the rails
to the ends--the ballast being only raised 2 inches in the middle of
the way, and sloped off so as to carry away the water under the rails.
From these observations it appeared that only five woods, Chella wungé,
Kara mardá, Palai, Karúvalem, and Ilupé, were sound at the end of two
years, the other eleven not lasting even that time. Also, that when the
sleepers were uncovered, decay was less rapid than when they were buried
in the ballast. The plan of leaving the sleepers partially uncovered had
many advantages; it effected a saving of the ballast, allowed the defects
to be more quickly detected, and kept the sleepers drier. It had been
urged that the heat of the sun would split the sleepers and cause the
keys and treenails to shrink; but from experience it was found that while
among the “uncovered” sleepers there was a large proportion “beginning
to split,” or “useless from being split,” there was on the other hand,
among the “covered” sleepers, a still larger proportion “beginning to
rot,” or “useless from being rotten.” It was also noticed that of the
sleepers “beginning to rot,” 19 per cent. had commenced under one or
both chairs. This was due to the retention of moisture under them, and
might be remedied by tarring the seats of the chairs. As regarded the
treenails where the sleepers were rotten, the treenails were invariably
found to be in the same state; while, when the heads were exposed to the
sun, they were not loosened by shrinking. Another objection was, that the
road would be more likely to buckle and twist, but this was not found in
practice to be the case. Treenails made in India cost 2_l._ 10_s._ to
4_l._ per 1000, and the woods generally used for the purpose are Vengé,
Kara mardá, Erul, Porasa, or satin wood, and Trincomalee. The three
woods first named are also extensively employed for keys, but teak keys
seem to be the best, and their cost does not exceed 6_l._ per 1000. From
the experience of the Indian engineers it appears that Teak, Saul, Sisso,
Pedowk, Kara mardá, Acha, Vengé, Chella wungé, Palai, Erul, Karúvalem,
will make very good sleepers to be used plain.

The sleepers which have failed on the Madras Railway might well be
divided into two classes,--those which were originally of perishable
woods, and were therefore unfit for the purpose; and those which although
of good wood had been cut from young trees, and not been allowed to
stand until old enough. The first arose from want of experience of the
nature of Indian woods: the second from the absence of a proper system of
working the jungles.

The wooden sleepers on the Indian railways should be tarred under the
seats of the chairs, be laid in dry ballast, and raised slightly in the
middle, and sloped off so as to throw the water under the rails. About
two-thirds of the Indian woods are practically useless owing to the want
of proper artificial means for preserving those of a perishable nature.

The subject of the decay of wood in India and tropical climates is too
extensive to be further considered here; but is of sufficient importance
to demand a volume to itself; the renewal of decayed wooden sleepers
to railways forming annually a most important item in foreign railway
budgets.

We have heard that some of our fortifications which have been erected
within the last few years to protect our English coast from invasion,
have already been invaded by dry rot. If this be true, some one well
acquainted with the subject should at once be appointed to find out the
cause, and recommend the remedy in each case.

Professional men, if they wish their works to “live for ever,” should
consider the after consequences of neglecting to provide against dry
rot. If the fungi could speak from under floors, ceiled-up roofs, behind
wainscots, girders, &c., we should often hear them exclaim, “A nice moist
piece of wood! Surely this belongs to us.” On the beams of a building at
Crawley, a carpenter many years ago cut a few words; they are full of
meaning in connection with our subject, and they run as follows:

“Man of weal, beware; beware before of what cometh behind.”

CHAPTER III.

FELLING TIMBER.

The end to be attained in the management of timber trees is to produce
from a given number the largest possible amount of sound and durable
woods. When a tree, under conditions favourable to its growth, ceases
increasing the diameter of its trunk, and loses its foliage earlier in
the autumn than it is wont to do, and when the top of the tree brings
forth no leaves in spring, these facts may be considered as indications
of decline, and that the tree is of sufficient age to be felled. The
state of the upper branches of a tree may be considered to be amongst
the best indications of its soundness, and provided they be in a
healthy condition, the withering of the lower branches is a matter of
comparatively small importance.

Trees may be considered as tall, middle rank, and low, and the size
to which they will attain depends on many different circumstances.
Some trees, the stems of which are short on the average, as the lime,
are virtually of tall growth, from the manner in which a number of
vertical branches of large size ascend from the stem. And other trees,
again, whose branches are comparatively short, are of tall growth, in
consequence of the length of the stems--like the beech.

The average duration of trees differs, as is well known, in different
species, and they exhibit different symptoms of decay. There are oaks in
Windsor Great Park, certainly nearly one thousand years old, and which
exhibit even now no appearance of approaching the end of their life. Mr.
Menzies, the surveyor, in his work on Windsor Great Park, describes some
of the indications of incipient decay which are peculiar to the several
kinds of trees. “When a beech begins to fail,” he says, “fungi appear
either at the roots or on the forks, the leaves curl up as if they had
been scorched, and the tree quickly perishes. In an elm, a great limb
first fails, while the rest of the tree continues green and vigorous,
but in a few years the whole tree suddenly dies. Coniferous trees die
gradually, but quickly. The oak shows the first symptoms at the points
of its highest branches, while the rest of the tree will remain healthy
and sound for years.” This peculiarity of the oak did not escape the eye
of Shakespere, that universal observer, who describes the monarch of the
woods as not only having its boughs mossed with age, but its

“High top bald with dry antiquity.”

The age for felling trees is a subject which calls for the deepest
consideration, but does not always receive that attention which is due
to its importance. Timber growers in their haste to supply the market,
too often fell trees that have not arrived at maturity, the heart-wood
being therefore imperfect, with much sap-wood, and, of course, little
durability; but unfortunately they are the more readily led to do so
on account of the increase in size being very slow after a certain
age. Builders are sensible of the inferior quality of young timber in
respect to duration, and it is their province to check this growing evil,
by giving a better price for timber that has acquired a proper degree
of density and hardness; but, unfortunately, this is an age for cheap
building, without much regard being given as to durability.

Felling should not be too early, for the reasons above mentioned; neither
should it be in the decline of the tree, when its elasticity and vigour
are lost, and the wood becomes brittle, tainted, and discoloured, with
the pith gone, and the heart in progress of decay. Maturity is the period
when the sap-wood bears a small proportion, and the heart-wood has become
uniform and compact. Sir John Evelyn writes, “It should be in the vigour
and perfection of trees, that a felling should be celebrated.” It must
be obvious, however, that it is a worse fault to fell wood before it has
acquired thorough firmness, than when it is just in the wane, and its
heart may exhibit but the first symptoms of decay; for in the former
there is no perfect enduring timber to be got, while in the latter the
greater part is in the zenith of its strength.

Although there are certain symptoms by which it may be ascertained when
a tree is on the decline, it is somewhat difficult to decide just when a
tree is at maturity. From the investigations of naturalists, however, it
may be safe to consider that hard-wood trees, as oak and chestnut, should
never be cut before they are sixty years old, the average age for felling
being from eighty to ninety years, and the average quantity of timber
produced by a tree of that age is about a load and a half, or about 75
cubic feet.

Daviller states (see ‘Cours d’Architecture’) “that an oak should not be
felled at a less age than sixty years.” Belidor considers (see ‘Sciences
des Ingénieurs’) “that one hundred years is the best age for the oak to
be felled.”

It should be remembered that the times mentioned are by no means
arbitrary, for situation, soil, &c., have much to do with it. For the
soft woods, as the Norway spruce and Scotch pine in Norway, the proper
age is between seventy and one hundred years. The ash, larch, and elm,
may be cut when the trees are between fifty and ninety years old; and
between thirty and fifty years is a proper age for poplars.

The felling of timber was looked upon by ancient architects as a matter
of much moment. According to Vitruvius, the proper time for felling is
between October and February, and he directs that the trees should be cut
to the pith, and then suffered to remain till the sap be drained out. The
effusion of the sap prevents the decay of the timber, and when it is all
drained out, and the wood becomes dry, the trees are to be cut down, when
the wood will be excellent for use. A similar effect might be produced
by placing the timber on its end as soon as it is felled, and it would,
no doubt, compensate for the extra expense by its durability in use. In
France, so long ago as 1669, a royal order limited the felling of naval
timber from the 1st October to 15th April, when the “wind was at north,”
and “in the wane of the moon.” Buonaparte directed that the time for
felling naval timber should be “in the decrease of the moon, from 1st
November to 15th March,” in order to render it more durable. In England,
in the first year of James I., there was an Act of Parliament prohibiting
every one from cutting oak timber, except in the barking season, under a
severe penalty.

James I. was not the only English sovereign who has been concerned with
timber trees; for King John was obliged to cancel at Runnemede the cruel
forest laws enacted by his father, William the Conqueror, especially
those restricting the people from fattening their hogs.

Up to a recent period large droves of hogs were fattened upon the
acorns of the New Forest in Hampshire. At the present time the hogs of
Estremadura are principally fed upon the acorns of the _Ballota_ oak; and
to this cause is assigned the great delicacy of their flesh.

A Berkshire labourer, living near Windsor Forest, thus speaks of the
delicacy of acorn-fed pork: “Well, that be pretty like the thing. I
hadn’t tasted the like o’ that this many a day. It is so meller--when you
gets your teeth on it, you thinks you has it; but afore you knows where
you is, ain’t it wanished!”

There is another point in connection with the time of felling timber,
which ought to be noticed. It is a widespread opinion that trees should
be felled during the wane of the moon. This planetary influence is open
to doubt, but the opinion prevails wherever there are large forests.
Columella, Cato, Vitruvius, and Pliny, all had their notions of cutting
timber at certain ages of the moon. The wood-cutters of South America act
upon it, so do their brethren in the German forests, in Brazil, and in
Yucatan. It was formerly interwoven in the Forest Code of France, and,
we believe, is so still. Vitruvius recommends this custom, and we find
Isaac Ware writing of the suggestion: “This has been laughed at, and
supposed to be an imaginary advantage. There may be good in following
the practice; there can be no harm: and therefore, when I am to depend
upon my timber, I will observe it.” The Indian wood-cutters believe that
timber is much more liable to decay, if cut when the moon is in crescent.

An American writer, in 1863, thus writes of his experience in the matter:
“Tradition says that the ‘old’ of the moon, in February, is the best
time to cut timber; but from more than twenty years of observation and
actual experience, I am fully convinced it is about the worst time to cut
most, if not all kinds of hard-wood timber. Birch, ash, and most or all
kinds of hard wood will invariably _powder-post_ if cut any time in the
fall after the tree is frozen, or before it is thoroughly leaved out in
the spring of the year. But if cut after the sap in the tree is used up
in the growth of the tree, until freezing weather again comes, it will
in no instance produce the _powder-post_ worm. When the tree is frozen,
and cut in this condition, the worm first commences its ravages on the
inside film of the bark, and then penetrates the wood until it destroys
the sap part thereof. I have found the months of August, September, and
October, to be the three best in the year to cut hard-wood timber. If cut
in these months, the timber is harder, more elastic, and durable than if
cut in winter months. I have, by weighing timber, found that of equal
quality got out for joiners’ tools is much heavier when cut and got out
in the above-named months than in the winter and spring months, and it
is not so liable to crack. You may cut a tree in September, and another
in the ‘old’ of the moon in February following, and let them remain, and
in one year from the cutting of the first tree, you will find it sound
and unhurt, while the one last cut is scarcely fit for firewood, from
decay. Chestnut timber for building will last longest, provided the bark
be taken off. Hemlock and pine ought to be cut before being hard frozen,
although they do not _powder-post_; yet if they are cut in the middle
of winter, or in the spring of the year, and the bark is not taken off,
the grub will immediately commence its ravages between the bark and the
wood. I have walnut timber on hand which has been cut from one to ten
years, with the bark on, which was designed for ox-helves and ox-bows,
and not a worm is to be found therein; it was cut between 1st August and
1st November. I have other pieces of similar timber cut in the winter
months, not two year’s old, and they are entirely destroyed, being full
of _powder-post_ and grub-worms.”

What shall we say when doctors disagree? The theory given to account for
what is assumed to be a fact, is, that as the moon grows the sap rises,
and the wood, therefore is less dense than when the moon is waning,
because at that time the sap in the tree diminishes. No evidence whatever
can be offered in support of the theory, and one would certainly imagine
that the rise or fall of the sap would depend on the quantity of heat
which reaches the foot of the tree, and not at all on attraction.

All investigations tend to prove that the only proper time for felling
timber is that at which the tree contains the least sap. There are two
seasons in each year when the vessels are filled. One is in spring, when
the fluid is in motion to supply nutriment to the leaves, and deposit
material for new wood; the other is in the early part of autumn, when,
after the stagnation which gives the new wood time to dry and harden, it
again flows to make the vegetable deposits in the vessels of the wood.
At neither of these times should trees be felled; for, if the pores be
full of vegetable juices, which being acted upon by heat and moisture may
ferment, the wood will decay. Of the two periods, the spring must be the
worst, because the wood then contains the greatest quantity of matter in
a state fit for germination.

The results of a series of experiments made in Germany show that
December-cut wood allows no water to pass through it longitudinally;
January-cut wood passed in forty-eight hours a few drops; February-cut
wood let two quarts of water through its interstitial spaces in
forty-eight hours; March-cut wood permitted the same to filter through in
two and a half hours. Hence the reasons why barrels made from wood cut in
March or April are so leaky, as the sap is then rising, and the trees are
preparing to put forth their leaves.

It thus happens that the time for felling is midsummer or midwinter. The
best time for felling, according to some, is midsummer, when the leaves
are fully expanded, and the sap has ceased to flow, and the extraneous
vegetable matter intended for the leaves has been dislodged from the
trunk of the tree by the common sap, leaving it in a quiescent state,
and free from that germinative principle which is readily excited by
heat and moisture, and if the timber were cut while it remained, would
subject it to rapid decay and to operations of worms. Midwinter, amongst
some, is chosen as a time for felling, as it is stated that winter-felled
heart-wood is less affected by moisture, and likely to be the best and
most durable; but as the only peculiar recommendation which that time
possesses is the facility which it affords for gradual seasoning, by
which timber is rendered less liable to split and get distorted, and
slow drying being generally available at any season under shade and
shelter, midsummer appears for many obvious reasons the most expedient.
In general, all the soft woods, such as elm, lime, poplar, willow,
should be felled during winter. In some kinds of trees a little after
midsummer appears to be decidedly the best time for felling. Alder felled
at that time is found to be much more durable; and Ellis observes, that
beech when cut in the middle of summer is bitter, and less liable to be
worm-eaten, particularly if a gash be cut to let out the sap some time
before felling. Mr. Knowles states that, “About Naples, and in other
parts of Italy, oaks have been felled in summer, and are said to have
been very durable.” Most of the trees in southern Italy are felled in
July and August, and the pines in the German forests are cut down mostly
in summer time, and it is stated that their wood is sound.

The following are advocates for winter felling, viz. Cato, Pliny,
Vitruvius, Alberti, Hesiod, De Saussure, Evelyn, Darwin, and Buonaparte.
Some of them consider that winter-felled timber, which has been barked
and notched in the previous spring, loses much of that half-prepared
woody matter, containing seeds of fungi, &c., that there is no doubt of
its superiority to summer-felled timber.

The age at which trees should be felled, and the most suitable time for
the work having been determined, there are two other things which claim
attention.

The _first_ of these is the removal of the bark from the trunk and
principal branches of the tree. For, in oak trees, the bark is too
valuable to be lost; and as the best period for the timber is the worst
for the bark, an ingenious method has been long partially practised,
which not only secures the bark at the best season, but also materially
improves the timber. This method consists in taking the bark off the
standing tree early in the spring, and not felling it till after the
new foliage has put forth and died. This practice has been considered
of inestimable value; for by it the sap-wood is rendered as strong and
durable as the heart-wood; and in some particular instances experiments
have shown it to be four times as strong as other wood in all respects
similar, and grown on the same soil, but felled with the bark on and
dried in sheds. Buffon, Du Hamel, and, in fact, most naturalists, have
earnestly recommended the practice. Evelyn states, “To make excellent
boards, bark your trees in a fit season, and let them stand naked a full
year before felling.”

In regard to the time that should elapse between the removal of the bark
and the felling of a tree, a variety of opinions exist. It was the usual
custom of early architects to remove the bark in the spring, and fell the
trees during the succeeding winter. Later investigations seemed to have
proved that it is better to perform the work three or even four years in
advance, instead of one, although Tredgold appears to think one year too
long. Trees will, in most situations, continue to expand and leaf out for
several seasons after the bark has been removed. The sap remaining in the
wood gradually becomes hardened into woody substance, thereby closing
the sap vessels and making it more solid. As bark separates freely from
the wood in spring, while the sap is in motion, it should be taken off
at that period. When the above method is not adopted, it is well either
to pierce the trunk some time before felling to drain out the sap, or
immediately on its being felled to set it on end.

The _second_ suggestion is, to cut into and around the entire trunk of
the tree, near the roots, so that the sap may be discharged; for in this
manner it will be done more easily than it can be by evaporation after
the tree is felled. In addition to this, if it be permitted to run out
at the incision, a large portion of the new and fermentable matter will
pass out with it, which would remain in the wood if only such material
is removed as would pass off by evaporation. This cutting should be made
in the winter previous to the August in which the tree is to be felled;
and the incision should be made as deep into the heart-wood as possible
without inducing a premature fall of the tree.

The custom of ringing or girdling the tree before felling has been
advocated, on the ground that the seasoning is thereby expedited,
and also more thoroughly effected. This is doubtful, at least, in
oil-containing trees (as teak, &c.), but the practice appears to be
contra-indicated for other reasons: when a tree has been ringed, many
wood-cutters object to cut it down on account of its increased hardness.
This objection might be waived, were it not for another and more serious
one which has been adduced. It is believed to be a fact by some that
trees felled after girdling have the heart shake increased. It is
difficult to explain this, if it be actually the case.

Many suggestions might be made as regards the mechanical operation of
felling trees, with which ancient nations were not unfamiliar:

… “for thou knowest that there is not among us any that can skill
to hew timber like unto the Sidonians.”--1 Kings v. 6.

But as these operations are familiar to all intelligent workmen, it
is only necessary to mention one, viz. the value of removing from the
side of the tree such branches as will strike the ground when it falls,
and, by wrenching, cleave the grain of the wood, and thereby injure the
timber. Such defects, which are often found after the timber has been
seasoned, could not be discovered when it left the mill.

In conclusion, we can truly state that the most extensive felling of
trees for _one building_ only which we have ever heard or read of is the
following:

“And Solomon had threescore and ten thousand that bare burdens,
and fourscore thousand hewers in the mountains.”--1 Kings v. 15.

CHAPTER IV.

ON SEASONING TIMBER BY NATURAL METHODS, VIZ. HOT AND COLD AIR; FRESH AND
SALT WATER; VAPOUR; SMOKE; STEAM; BOILING; CHARRING AND SCORCHING, ETC.

All timber must, whether it be sap-wood or heart-wood, be placed in
situations which will allow the sap to exude or evaporate, and this
process is the one technically known by the term “seasoning.” There are
natural and artificial modes of seasoning, both of which have their
recommendations; but the former has certainly the right of preference,
as it gives greater toughness, elasticity, and durability, and therefore
should always be employed in preparing timber for carpentry. As the word
“timber” has been frequently used, it may be as well to state that it is
derived, according to Dr. Johnson, from the Saxon, _timbrian_, to build:
hence the above definition. The legal definition of timber is restricted
to particular species of wood, and custom varies in different countries
as to the species ranked among the timber trees.

When a tree is felled, it encloses in its fibres as well as in capillary
channels a considerable quantity of sap, which is nothing else but water
charged with gummy, saccharine, saline, mucilaginous, and albuminous
matters. In this state, the latter are very liable to ferment, but they
lose their liability when, by the evaporation of the sap, they pass
to a dry and solid state; so that the first suggestion which naturally
presents itself to the mind, is to subject the timber to a lengthened
seasoning.

But the present demands for time will not admit of this, and therefore it
is imperative to resort to artificial and speedy methods.

With respect to the value of timber in the log, owing to its becoming
rent by the weather, it sells for 15 per cent. less the second year than
the first, and so on for less and less the longer you keep it.

A natural seasoning may be adopted for specimens of moderate thickness,
such as deals, planks, &c. At the end of eighteen months from the time of
importation they are scarcely dry enough for the consumer’s use.

When there is time for drying it gradually, all that is necessary to be
done on removing it from the damp ground of the forest, is to place it
in a dry yard, sheltered from the sun and wind, and where there is no
vegetation; and set it on bearers of iron or brick in such a manner as to
admit of a ventilation all round and under it. In this manner it should
continue two years, if intended for carpentry; and double that time,
if intended for joinery; the loss of weight which should take place to
render it fit for the purposes of the former being about one-fifth; and
for the latter about one-third. In piling it, the sleepers on which the
first pieces are laid should be perfectly level, and “out of the wind,”
and so firm and solid throughout that they will remain in their original
position; for timber, if bent or made to wind before it is seasoned,
will generally retain the same form when dried. Blocks of wood should
be put between the “sticks” of timber, and each piece directly over the
other, so that air may freely pass through the whole pile; for while it
is necessary to shield timber from strong draughts of wind and the direct
action of the hot sun, a free circulation of air and moderate warmth are
equally essential.

[Illustration: PLANS OF DIFFERENT BALTIC MODES OF CUTTING DEALS FOR THE
ENGLISH AND FRENCH MARKETS.

THE SMALLEST TREES ARE CUT FOR DEALS; THE LARGEST FOR LOGS.

OLD MODE OF CUTTING.

ENGLISH BATTEN. 7IN × 2½IN
ENGLISH DEAL. 9IN × 2½IN
ENGLISH DEAL. 9IN × 2½IN
ENGLISH BATTEN 7IN × 2½IN
9 × 2½ = 22½ × 2 = 45in
7 × 2½ = 17½ × 2 = 35/80

MODE PRACTISED UNTIL THE FRENCH MARKET IMPROVED.

ENGLISH BATTEN. 7IN × 2½IN
ENGLISH DEAL. 9IN × 3IN
ENGLISH BATTEN. 7IN × 2½IN
9 × 3 = 27 = 27in
7 × 2½ = 17½ × 2 = 35/62

MODE GENERALLY ADOPTED AT THE PRESENT TIME.

FRENCH DEAL. 9IN × 1¼IN
ENGLISH DEAL. 9IN × 3IN
ENGLISH DEAL. 9IN × 3IN
FRENCH DEAL. 9IN × 1¼IN
9 × 3 = 27 × 2 = 54in
9 × 1¼ = 11¼ × 2 = 22½/76½

_Notes on Deals._

_All deals are liable to dry rot, if placed in contact with damp
brickwork._

_If the pith of a tree be left in the centre of a deal, dry rot attacks
it._

_Dry rot first attacks the sapwood of a deal; and next, the pith._

_Stockholm, or Gefle deals are not liable to be affected with dry rot._

“STRONG” DEALS _rend. When sawn, they do not give saw dust, but the
fibres tear_.

BEST DEALS _are light, mellow, and exhibit a silky texture when planed_.

“BESTS”. _Wholly free from knots, shakes, sapwood, or cross grain, and
well seasoned._

“SECONDS”. _Free from shakes, and sapwood: small knots allowed._

“THIRDS”. _All that remains after “bests” and “seconds” have been picked
out._]

If timber is not used round, it is good to bore out the core; as, by so
doing, the drying is advanced, and splitting prevented, with almost no
sacrifice of strength. If it is to be squared into logs, it should be
done soon after some slow drying, and whole squared, if large enough, as
that removes much of the sap-wood, facilitates the drying, and prevents
splitting, which is apt to take place when it is in the round form, in
consequence of the sap-wood drying before the heart, from being less
dense. If it may be quartered, it is well to treat it so after some time,
as the seasoning is by that means rendered more equal. It is well also to
turn it now and then, as the evaporation is greatest from the upper side.
In France, the term “bois du brin,” means timber the whole size of the
tree, excepting that which is taken off to render it square.

To prevent timber warping to any serious extent, it should be well
seasoned before it is cut into scantlings; and the scantlings should be
cut some time before they are to be used, in order that the seasoning
may be as perfect as possible; and if they can be set upright, so much
the better, as then they will dry more rapidly. The white lowland deals
of Norway and the white spruce deals of Canada have the same disposition
to warp and split on drying. Du Hamel has shown that it is a great
advantage to set the timber upright, with the lower end raised a little
from the ground; but as this cannot always be done, the timber-yards
should be well drained and kept as dry as possible. “Ancient architects,”
observes Alberti, “not only prevented the access of the scorching rays of
the sun and the rude blasts of wind, but also covered the surface with
cow-dung, to prevent the too sudden evaporation from the surface.” The
warping of timber is attributable by some to the manner of its growth.
Boards cut out of a tree that is twisted in its growth will not keep
from warping; boards cut from trees that are grown in open situations
have another fault, in the heart of the tree not running straight like
forest-grown wood. In a plank cut from a tree of this kind in a straight
line, the heart will traverse it from one end to another. No treatment
will prevent it from warping or drying hollow on the side farthest from
the heart. Where the heart is in the centre of a plank, and each side has
an equal chance of drying, it will not warp; but there will be a shake or
crack upon each side, denoting the position of the heart.

Some deals, and particularly the stringy deals, are very hygrometric,
and never lose the property, however long they have been seasoned, of
expanding and contracting with change of weather. White Petersburgh deals
are said to have that property, however long they may have been kept,
so that if used in the panel of a door, the wood alternately enters and
recedes from the groove into which it fits, as the paint will show when
that kind of deal has been used for a panel.

The wood of the north side will not warp so much as the wood from the
south side. The face of the planks should be cut in the direction which
lay from east to west as the tree stood. If this be done, the planks will
warp much less than if cut in the opposite direction. The nature of the
tree, the soil upon which it is grown, the position of its growth, the
period of the year in which it is felled, and the length of time between
its felling and converting, are the principal points to be considered; a
thorough knowledge and study of which is the only true principle on which
we can hope to deal with the warping and converting of timber.

Wood, when it is cut into small pieces, very soon acquires its utmost
degree of dryness. Dr. Watson, Bishop of Llandaff, in the month of
March, cut a piece from the middle of a large ash tree that had been
felled about six weeks, and weighed it; its weight was 317 grains. In
seven days it lost 62 grains, or nearly one-fifth of its weight. It was
weighed again in August of the same year, but had not lost any more of
its weight; hence it had become perfectly dry in the short space of seven
days. He also found that the sap-wood of oak lost more weight in drying
than the heart-wood, in the proportion of 10 to 7.

The time that is required to season or dry a piece of timber obviously
depends upon its magnitude; as a _general rule_, large timbers will not
continue good so long as small ones, as sufficient time is rarely given
for a thorough seasoning. The time required to dry a piece of timber, all
other things being alike, will depend on the quantity of surface exposed
to the action of the air; therefore, while the quantity of timber
remains the same, the larger the surface, the sooner it will dry. Also,
if the quantity of surface remains the same, the time of drying will be
proportioned to the quantity of matter; as the greater the quantity of
matter under the same surface, the longer it will be in drying.

As drying proceeds most rapidly in small pieces, it is therefore
important to reduce the timber to its proper scantlings or size for
use; for however dry a piece of timber may be, when it is cut to a
smaller scantling it will shrink and lose weight, being always less dry
in the centre than at the surface; and the more rapidly the drying has
been carried on, the greater will be the difference. Nevertheless, in
the first stage of seasoning it is best that it should proceed slowly;
otherwise, the external pores shrink so close as not to permit the
full evaporation of the internal moisture, and the piece would split
from unequal shrinking; and lastly, it should be reduced to the proper
scantling, as already observed, some time before it is to be framed.
Various tables have been given by writers on timber, the result of
algebraical calculations, of the times of seasoning and drying for
different woods of different lengths, breadths, and thicknesses, in the
open air; but as wood even of the same description and quality varies
so much, this matter is best left to those who are well acquainted with
timber. It may, however, be stated that the time required for drying
under cover is shorter than in the open air, in the proportion of 5 to 7.

The English shipwright considers that three years are required to
thoroughly season timber. The timbers for ships are usually cut out
to their shape and dimensions for about a year before they are framed
together, and they are commonly left a year longer in the skeleton shape
to complete the seasoning, as in that condition they are more favourably
situate as regards exposure to the air than when they are closely covered
in with planking.

It is worthy of mention that all the harder woods require increased care
in the seasoning, which is often badly begun by exposure to the sun or
hot winds in their native climates: their greater impenetrability to
the air the more disposes them to crack, and their comparative scarcity
and expense are also powerful arguments on the score of precaution. Oak
timber requires to be very carefully seasoned, as it is generally used
in buildings for the best description of work, and should unseasoned oak
be used for “panelling,” any shrinkage will be fatal to the work. Mr.
George Marshall, timber merchant (see the _Builder_, January 20, 1872),
with respect to seasoning oak timber, observes: “I should select oak
trees known to be old and hearty, with clean, straight butts, from 15
inches to 20 inches in diameter. I should then have the bark taken off
as they stand, and leave them thus till the winter; the sap will then
partially dry out, and make the wood a rich brown colour. As soon as they
are cut down, have them sawn up at once into the lengths you require the
panelling, 6 inches or 8 inches wide and 1 inch to 1½ inch thick. Be
careful to cut all the heart shakes, by having one cut through the centre
of the log before edging the boards to the required width. With regard
to the drying process, stack the boards in a shed with a good draught
through it, and load them down, with slips between each board, to prevent
warping. If this be done they will be found to dry well and speedily, and
they will not require to be exposed to the weather.”

Sir. Robert Phillips, on seasoning oak for panelling, states: “If the
tree is large enough for the purpose, cut it into four, in sections, by
drawing a vertical and horizontal line across the end, meeting in the
centre. If too small for this, cut it into 4½ inch or 6-inch plank, as
soon as possible after felling, and then stack _on end_ out in the open:
do not lay on the ground, but stand it as nearly _vertical_ on its end as
possible, and keep it wet during the first three months. If the weather
is dry, well _wet_ it with water poured on the top, and allowed to run
down. Let the ends stand on a piece of quartering, to keep it out of the
dirt, or it will be stained some distance up. After standing thus for
some six months, after putting it in a dry place for some time, cut it
into the scantlings you require, always bearing in mind that oak will,
after this seasoning, shrink at least half an inch to a foot, in width
and thickness. They should then be stacked and stripped, and covered with
spare boards, and weighted on the top, for at least six months--as much
more as possible--in a covered shed, with plenty of air, occasionally
turned over and shifted, till they are dry enough to make dust when
planed, and not turn the shaving black. They will then be fit for use.

“I should advise for the panels to be cut _feather-edged_ boards, in
radial lines from the centre of the tree: it will be a waste of material,
but will repay in the beauty of the wood, and the way it will stand
without warping. Most of the panels of our old cathedrals were rent (_not
sawn_) in this way, and stand admirably. The butt of the tree should be
taken, the top being used for a rougher purpose.”

Mr. George Marshall and Mr. Robert Phillips might have mentioned that
the oak trees should be of the _Quercus Robur_ species, and _not_ the
_Quercus Sessiliflora_. They are easily distinguished when growing by the
following peculiarities: The acorn-stalks of the _Robur_ are _long_; the
acorns grow singly, or seldom two on the same footstalk; the leaves are
_short_. The acorn-stalks of the _Sessiliflora_ are _short_; the acorns
grow in clusters of two or three, close to the stem of the branch; the
leaves are _long_.

WATER SEASONING.

When there is not time for gradual drying, the best method, perhaps,
that can be adopted, especially for sappy timber, and if strength is not
principally required, is immediately on felling to immerse it in running
water; and after allowing it to remain there about a fortnight, to set
it in the wind to dry. Some persons prefer this method of seasoning
timber, as they say it prevents cleaving, and strips and seasons better
afterwards. This process has been adopted with good results by placing
the boards end on at the head of a mill race for fourteen or twenty days,
at most, and then setting the boards upright, and subject to the action
of the sun and wind; though it is questionable whether the sun will not
do them more harm than good. As they stand, turn them daily, and when
perfectly dry--which process will take about one month--it is considered
they will be found to floor better than timber after many years of dry
seasoning. The sap-wood of oak is said to be improved by this method,
being much less subject to be worm-eaten; and providing it is placed in
fresh running water, Mr. G. A. Rogers, the celebrated wood carver, is of
opinion that the colour of the oak is improved. The more tender woods,
such as alder and the like, are less subject to the worm when water
seasoned. Beech is said to be much benefited by immersion. It should be
remembered that the timber should be altogether under water (chained
down beneath its surface), as partial immersion is very destructive. Du
Hamel considers “that where strength is required, wood ought not to be
put in water.” Timber should never be kept floating in ponds or docks,
as in London; but it should be stacked, as at Liverpool and Gloucester.
Timber that has been lying for months in ponds or docks is sometimes cut
up, and in six or seven days fixed in a building; consequently, the usual
result takes place, viz. dry rot. After having been swelled by soaking
much beyond its former bulk, the baulk of timber is put on the saw-pit,
and cut into scantlings, and framed while in this wet state, therefore
it cannot be surprising that the dry rot soon appears as a natural
consequence.

Amongst wheelwrights the water seasoning is in general favour. It is
said that the colour of the white woods is improved by water seasoning,
boiling, or steaming. The Venetians place the oak used for gun-carriages
in water for two years before it is used, and the timber for sea service
two or three years under water. The Turks do not appear to pay any
attention to seasoning, for they fell their timber at all times of the
year without any regard to the season, and although they grow very good
oak, it is used so green and unseasoned that it not only twists, but
decays rapidly, as anyone may observe in the houses at Constantinople and
other Turkish towns.

Timber is rendered more durable by placing it in a stream of water,
saturated with lime, for eight or ten days, and it also makes it less
liable to the attack of worms; but it, however, becomes hard after being
dried, and is difficult to be worked; and therefore the process should
be applied to timber which has been sawn into scantlings, and is ready
for use. Mr. William Chapman, in 1812, considered that an immersion of
timber in hot limewash in deep ponds, exposing little surface to the air,
merited a trial; but in 1816, from experiments he had made, he was of
opinion that it had proved injurious to timber.

Evelyn states that green elm, if plunged for a few days in water
(especially salt water), obtains an admirable seasoning. According to
Society of Arts _Trans._, 1819, every trace of fungus was eradicated from
the ship “Eden,” by its remaining eighteen months under sea water. Salt
water is considered good for ship timber, but for timber to be employed
in the construction of dwelling-houses, fresh water is better. Pliny
notices, as a fact, that certain woods on being dried after immersion in
the sea acquire additional density and durability. M. de Lapparent, late
Director of the French Navy, considers that timber cannot be seasoned
in salt water, but in fresh, or at the most, in brackish water. The
condition of the timber which, at the port of Rochefort, is kept in
ditches filled with fresh water is in this respect most favourable; that
kept at Toulon, Brest, and Lorient, where the water is brackish, is much
less so; but to estimate their relative advantages, it would be necessary
to test the average density of these waters. It is, however, at Cherbourg
that this natural preparation of timber is the most inefficient, as the
beds-of sand in which the timber is buried, near the Pool of Tourlaville,
contain but a small quantity of water, which, being nearly always
stagnant, very quickly exhausts itself, and is very prejudicial.

At the Cologne International Agricultural Exhibition, in 1865, three
sleepers were exhibited from the Magdeburg Leipsiger Railway, from the
Salt Work Branch, at Stassfurt, laid in 1857. These were moistened by the
refuse of the salt which was lost from the load and by the rain. The jury
in their Report stated that these sleepers proved nothing, “because every
old table on which fish or meat has been salted, proves that a constant
moistening with salt water preserves the wood from decay, but as soon
as the process of salting is given up, the salted matter is immediately
given out, and the timber soon decays. In this case it would have been
important to have known that these sleepers, after having been salted,
had lain anywhere else than in the Salt Work Branch without getting fresh
salt applied, and then to have seen if they would have been as perfect as
they are now. They, indeed, prove nothing but the fact that if sleepers
be daily sprinkled with salt they will remain sound, but the price paid
for this durability might be very considerable.” As the use of salt as
a preservative agent will be considered in the next chapter, it will be
best to defer the consideration of salt-water seasoning until then.

In India, teak, sál, and blackwood, &c., improve by lying in water, or
in the soft black mud of an estuary: there is one exception, viz. heddé,
which deteriorates from steeping, and should be carted to its destination.

Evelyn states that he had found a fortnight’s immersion in river water
sufficient, and this opinion is held by Silloway, a North American
authority; but Dr. Porcher, a South American writer, recommends a six
months’ immersion in water, and a six months’ exposure to wind and shade.
Vitruvius and Alberti consider that timber should be left immersed in a
running stream thirty days.

It is considered that the longer wood has remained under water, the more
rapidly it dries; for instance, every one is aware that the firewood
brought out of the river is less green and burns better than that brought
by waggon or boat.

In 1817, Admiral Count Chateauvieux, a Sardinian naval officer, observed
to Mr. McWilliam that it was a custom at the Royal Arsenal, at Genoa,
as a preventive against the diseases of timber, to steep it about three
years in fresh water immediately after it is felled. Mr. James Dickson,
of Gottenburg, timber merchant (member of the firm Peter Dickson and
Company, London), many years engaged in the Swedish timber trade,
observed in 1835, “If square timber lies in the water two or three years,
it rends at the heart, but I should not say it would, perhaps, for the
first year; but the exterior part rends soon by exposure to the weather.”
In 1818, the Chevalier de Campugano, Secretary of Legation to the Spanish
Embassy, stated that in Spain, when timber is felled, it is generally
laid in water for a considerable time.

The sap in timber, by reason of the matters which it holds in solution,
is denser than pure water; moreover, it is enclosed in fibres or channels
permeable at the ends.

Supposing in submerged timber, the surrounding water to be flowing, or at
least changing, this water will conclude by occupying, if not altogether,
at least in a great degree, the place of the sap, which will have issued
forth, carrying with it the fermenting principle with which it is
charged. The timber, therefore, which has remained _sufficiently long_
in the water ought to be much less susceptible of fermentation than that
seasoned only by the atmosphere. Besides, as pure water evaporates much
easier than that which contains certain principles, this timber ought to
be seasoned much sooner than the other.

Of steeping generally, whether in cold or warm water, it must be
particularly observed that it dissolves the substance of the wood, and
necessarily renders it lighter; indeed, it is known that notwithstanding
wood that is carefully submerged remains good for a very long period
after the water has dissolved a certain soluble part, it is, when taken
out and dried, liable to be brittle, and unfit for any other work but
joinery.

SEASONING BY STEAMING AND BOILING, ETC.

For the purposes of joinery, steaming and boiling are very good methods,
as the loss of elasticity and strength which they produce, and which
are essential in carpentry, is compensated by the tendency to shrinkage
being reduced; the durability also is said by some to be rather improved
than otherwise, at least from steaming. If steaming be not carried on
too quickly it will answer, but if it be pushed with too much vigour
it is very apt to produce a permanent warping and distortion of the
material. Oak of British growth may be seasoned by this process, as
without this precaution it requires a long time to season. It has been
ascertained, that of woods seasoned by these methods, those dried soonest
that had been steamed; but the drying in either case should be somewhat
gradual, and four hours are generally sufficient for the boiling or
steaming process. The question of time will depend upon circumstances:
some persons consider that one hour should be allowed for every inch
in thickness. In some dockyards, salt water is used in the boilers, in
others fresh, from considerations of convenience; and the fact is, plank
boiled in salt water never gets rid of the salts that naturally enter the
pores of the wood in boiling; and such being the case, the ship in which
this plank is used is much more liable to the effects of damp than she
would have been if the plank had been boiled in fresh water.

Boiling and steaming are likewise employed for softening woods, to
facilitate the cutting as well as bending of them. Thus, in Taylor’s
patent machines for making casks, the blocks intended for the staves are
cut out of white Canada oak to the size of 30 inches by 5 inches and
smaller. They are well steamed, and then sliced into pieces ½ inch or
⅝ inch thick, at the rate of 200 in each minute, by a process far more
rapid and economical than sawing; the instrument being a revolving iron
plate of 12 feet diameter, with two radial knives arranged somewhat like
the irons of an ordinary plane or spokeshave.

How far steaming or boiling affects the durability of timber has not been
satisfactorily ascertained; but it is said that the planks of a ship
near the bows, which are bent by steaming, have never been observed to
be affected with dry rot. With respect to boiling, Du Hamel’s opinion is
not favourable as to its adding to the durability of timber; for when a
piece of dry wood was immersed in boiling water, and afterwards dried in
a stove, it not only lost the water it had imbibed, but also a part of
its substance; and when the experiment was repeated with the same piece
of wood, it lost more of its substance the second time than it did the
first. Tredgold--no mean authority--considers that “boiled or steamed
timber shrinks less, and stands better than that which is naturally
seasoned.” Barlow is of opinion that “the seasoning goes on more rapidly
after the piece is steamed than when boiled.”

At the close of the Crimean and Baltic campaigns the port of Cherbourg
was almost completely cleared of staves sufficiently seasoned for making
casks. The engineer at the head of the coopering department determined to
boil in fresh water the newly-cut staves, and compare the time of their
seasoning with that of other staves cut from the same forests, but not
prepared; and the result was that after four or five months’ exposure
to the atmosphere, the boiled staves were perfectly fit for working up,
while to bring the others to the same point fifteen months were barely
sufficient.

Steaming is understood to prevent dry rot. No doubt boiling and steaming
partly remove the ferment spores, but _may not_ destroy the vitality
of those remaining. For, according to Milne-Edwards, on ‘Spontaneous
Generation.’ he has seen tardigrades resist the prolonged action of a
temperature of 248° Fahr., and has known them to survive a temperature of
284° Fahr. That low forms of vegetation are fully as tenacious of life
cannot be doubted.

Boiling and steaming also coagulate the albumen at 140° Fahr. Although
coagulated albumen is insoluble in water, the water solution is by this
heating process sealed up in the wood, and the cohesion of the latter is
said to be diminished.

The first essays in the art of drying wood artificially carry us back to
a period now tolerably remote. Wollaston and Fourcroy both recommended
the drying of wood in ovens. Newmann, a German chemist, suggested another
method, which has since been adopted in a somewhat different form, i.
e. _steaming_ the wood. Newmann placed the wood to be dried in a large
wooden chest, taking care to leave spaces between the pieces, and then
turned on the steam from a boiler provided for the purpose. The condensed
steam, charged with albuminous matter taken up from the wood, or rather
from its surface, was run off from time to time, and the process of the
operation was judged by the colour of the water. When the latter was
clear and colourless the chest was opened, and the wood withdrawn for use
without further preparation. The process would have been useful enough
if _superheated_ steam, which would have dried the wood by absorbing
the moisture, could have been used, but the cost of the process would
doubtless have been too high to permit of its practical application.

In 1837, M. de Mecquenem devised a method of desiccation, in which the
pieces of wood to be dried were placed in a closed chamber, and subjected
to a current of hot air, heated for the purpose by a special apparatus,
and driven by a blower. The air entered by apertures in the lower part
of the chambers, and escaped at the top laden with the moisture absorbed
from the wood.

In 1839, M. Charpentier obtained a _brévet d’invention_ for a process of
drying wood in hermetically-closed chambers. The wood was subjected to
the action of air heated by contact with metal plates covering the flue
of a coke furnace. This air entered by conduits on the level of the floor
of the chamber, and escaped at the top through apertures leading into the
chimney of the furnace.

In the same year, M. Saint Preuve invented a process for forcing steam
into pores of the wood, and, by condensation of this steam in the pores,
sucking in a preservative preparation.

In 1847, MM. Brochard and Watteau’s process was introduced. It consists
simply of filling the cylinder with steam, and making a vacuum by forcing
in a cold solution of salt, &c.

The plan which has been for some years in use in England is the
injection, by means of a ventilator, of hot air into the drying stove
where the wood is placed: by this the temperature is gently and gradually
raised until it reaches boiling heat. But, as wood is one of the worst
conductors known of caloric, if this plan is applied to large logs, the
interior fibres still retain their original bulk, while those near the
surface have a tendency to shrink; the consequence of which would be
cracks and splits of more or less depth.

Timber may be dried by passing rapid currents of heated air through it
under pressure. This plan was carried out with the timber used for the
floorings of the Coal Exchange, London. The wood was taken in its natural
state, and in less than ten days it was thoroughly seasoned. In some
cases, from 10 to 48 per cent. of moisture was taken out of the wood,
and although the floorings have now been down a great many years, it is
stated that very little shrinkage has been found, except in the case of
a few pieces which were put down in the latter portion of the work, and
which had not been submitted to the seasoning process.

The process of desiccation, patented by Messrs. Davison and Symington,
in 1844, is of great practical value in reducing the time requisite
for seasoning timber. It is peculiarly applicable to the seasoning of
flooring boards and of the wood used in joiners’ work. Care must be
exercised when removing the timber from the stove to the building in
which it is to be used, that it be not exposed to the wet, nor even to a
damp atmosphere for any lengthened period. The advantage of this process
over the ordinary stoving consists in the temperature never being so
high as to scorch the wood, by which the strength of the fibres would
be injured; and in the facility for removing the vapour as fast as it
is expelled from the wood, in consequence of the air being propelled
through the stove at any required velocity and temperature. As compared
with furnace and steam-stoving ordinarily employed to desiccate woods,
the great superiority of this process is established by its seasoning
the wood quite as rapidly, but much more thoroughly; and instead of wood
being rendered brittle, as it is to some extent by stoving, this mode
does not reduce the strength and tenacity of the wood. The principle
of the invention is propelled currents of heated air; but the heat
has to be regulated according to the texture of the various woods.
Honduras mahogany might be exposed to a heat of 300°, and the whole of
the moisture can be taken out in three days. Timber 9 inches square is
considered by Mr. Davison a proper size for his invention. This process
is described as “A method or methods of drying, seasoning, and hardening
wood, and other articles, parts of which are also applicable to the
desiccation of vegetable substances generally.” The first or principal
part of the invention consists in drying, seasoning, and hardening wood
and other articles--among which other articles are included generally all
things made of wood, or chiefly of wood--by means, as has been stated,
of rapid currents of heated air. The manner in which these currents of
heated air are produced, is by an apparatus consisting of a furnace
and a series of pipes withinside of a core of brickwork. On each side
of the furnace, on a level with the fire-bars, is a horizontal tube;
communicating and springing from these tubes are a series of eighteen
tubes placed vertically and parallel to each other over the furnace. The
outer end of one of the horizontal tubes communicates with a fan or other
impelling apparatus for driving a constant stream of atmospheric air
through the tubes. As the air passes through the tubes it becomes heated
at a high temperature, and rushes out at the farther end of the other
horizontal tube, and is thus conveyed to the place where it is applied.
The materials to be subjected to the heated currents, such as logs,
deals, &c., by outward application, must be placed in closed chambers,
galleries, vaults, or flues, which are to be of any suitable form or
magnitude; but it is recommended that they should be made of fire-brick,
and have double doors or shutters for introducing or removing the wood.
Honourable Mention was made of Messrs. Davison and Symington’s process of
desiccation, by the jury, Class IV., Exhibition of 1851, England.

Some amusing instances are related of the efficiency of Davison and
Symington’s process. Thus, a violin had been in the owner’s possession
for upwards of sixteen years; how old it was when he first had it is
not known. Upon being exposed to this process it lost, in eight hours,
no less than five-sixths (nearly five and two-thirds) per cent. of its
own weight. This there is every reason to believe was owing to the
blocks glued inside, for the purpose of holding the more slender parts
together. A violin maker of high reputation, having an order to make
an instrument for one of the first violinists of the day, was requested
to have the wood seasoned by this process; only three days were allowed
for the experiment, in which the wood was seasoned and sent home. The
two heaviest pieces were reduced in weight 2½ lbs. It is ascertained
that, by this means of drying, the effect of age has been given to the
instrument made from the above wood, and it was, in 1848, _first fiddle_
in the orchestra of Her Majesty’s Theatre, London. The wood had been
in the possession of its owners for eight years, and it was sent from
Switzerland, in the first instance, as _dry wood_.

In proof of the value of this invention for the manufacture and cleansing
of brewers’ casks, it was stated, in 1848, that since its adoption at
Trueman’s brewery, Spitalfields, a saving of 300 tons of coals has been
effected annually.

Flues or chambers for the heated air may be constructed in parallel
lines, either in the floors or upright walls of a building, having narrow
openings through which the heated air may issue in thin streams, and
spread itself over the surface of the wood. If the openings are in the
floor, the wood will require to be placed in an upright position; but if
admitted in a horizontal direction, standards and skeleton shelves will
be necessary to lay it upon. The great object, in all cases, is to bring
the heated air as speedily as possible into contact with the wood, and to
allow it, after it has done its office, to pass away as speedily.

Furnaces and apparatus for the production of rapid currents of heated
air may be erected to prepare any quantity of timber or articles of wood
at one time, but care should be taken that whatever the size of the
outlet may be from the series of pipes or vessels by which the heat is
generated, an outlet of at least equal dimensions is left for the free
exit of the air and the vapours thrown off. It should also be observed,
in constructing the open space in the floor or upright walls for the
stream of heated air to pass towards the timber, that the superficial
area of the whole of them combined does not exceed the dimensions of the
principal outlet of the pipes at the extremity of the furnace, so that a
free current of heated air may be allowed to pass uniformly throughout
the chambers containing the wood to be prepared. The temperature proper
to be given to the air, and velocity to the current in each case, will
depend on the size, density, and maturity of the wood to be acted upon.
The inventors found by their experiments that wood generally may be
advantageously subjected to currents of air raised to a temperature of
400° Fahr., when the currents are impelled at the rate of 100 feet per
second. But when the wood is in a green state, it is better to commence
at a lower temperature, say from 150° to 200°, and gradually raise it to
the high degree before stated, as the desiccation proceeds, an object
which may, in some cases, be facilitated by carrying a cold-air drain
from the fanner or other propelling apparatus, and attaching a damper to
it, so that any quantity of cold air required to reduce the temperature
of the hot current may, from time to time, be admitted. When, again, the
wood is in the log or unconverted state, it should be bored or augured
out in the centre, and the current of hot air caused to traverse it as
well interiorly as exteriorly, whereby much time will be saved in the
process of desiccation, and a more uniform result obtained.

Woods treated in this manner, and with the above modifications when
requisite, part rapidly with their natural sap and any other aqueous
matter which they may contain, and the fibres are brought closer together.

With respect to the time required to season the wood upon this plan, much
must depend upon the original state of dryness it may be in, as well
as the quality and temperature of the heated air forced into contact
with it. It may suffice to remark that the wood may safely remain thus
exposed till any escape of moisture ceases to be perceptible. This may be
readily known, either by applying a mirror or any polished surface to the
outlet, or by calculating the quantity of moisture removed from the wood,
which will be found to range between ¼ and ⅟12th of its whole weight.
For the purpose of ascertaining more correctly the amount of moisture
removed from time to time, when the wood is placed in seasoning chambers
as already described, an opening should be constructed in the chamber,
in any convenient position, through which a specimen of the wood may be
withdrawn and weighed.

Between 1848 and 1853, Mr. Bethell, who had paid much attention to the
subject, obtained several patents, both in England and France, for stoves
for drying wood. In his English patent of 1848, and the subsequent French
one of 1853, we find a description of a peculiar kind of stove, on the
following plan:

It consisted of a rectangular chamber formed of three walls and vaulted
over, the whole in brickwork, with a certain thickness of slag in the
centre, to prevent loss of heat. One extremity of the chamber was open to
admit of the introduction of the wood by means of a truck running upon
longitudinal iron rails. The opening was closed with a double door when
the chamber was full. On the exterior of the opposite end of the chamber
was a furnace to burn coal, coke, wood, or tar, according as it was
desired to _dry_ the wood simply, or, in the words of the inventor, to
_smoke_ it, i. e., to impregnate it with the antiseptic gaseous matters
evolved in the imperfect combustion of certain tarry substances. The
heated air or smoke entered through a flue running along the floor and
branching at the end, and it escaped, or was pumped out, at the top of
the vaults. Bethell considered that the interior of the chamber should be
kept at a temperature of 110° Fahr., and that the duration of the process
should be regulated by the condition of the wood. His experiments showed
that this time varied from eight to twelve hours, the rapidity being
attained at the cost of a relatively large expenditure of fuel. In point
of fact, the draught was too great to permit of the utilization of the
full amount of heat contained in the gaseous matter, which escaped at a
temperature very little below that at which it entered. The heat produced
by the fuel was badly utilized, and it is open to question whether,
under any circumstances, large pieces of wood, such as sleepers, could
be dried in so short a time as eight or twelve hours. The drying could
only be effected by the use of a very high degree of temperature, tending
to split the wood and weaken its strength. This view was confirmed by
the results obtained in a long series of experiments made, in 1852-3,
by an English manufacturing company, known as the Desiccating Company. A
low temperature, and long continuance of the drying process, appear to
be the conditions essential to the success of artificial desiccation,
particularly with wood intended for cabinet-making, turning, joinery,
ornamental work, &c., in which it is desirable, as far as possible,
to prevent splitting, warping, and other changes of structure in
the material. These results, it would seem, were not secured by the
arrangements above described.

Some years since, a stove was constructed for Messrs. S. and J. Holme,
very extensive builders at Liverpool, for the purpose of drying timber
for floors, and other fittings of houses, &c., by the application of
Messrs. Price and Manby’s patent warming apparatus; the want of seasoned
timber, with the great number of men they employed, being a serious
inconvenience and loss. In their large undertakings Messrs. Holme found
a difficulty in keeping a stock of dry timber. The dimensions of the
stove in which the timber was to be dried was 43 feet long, 11 feet
wide, and 17 feet 6 inches high, and the cost of the apparatus was about
150_l_. It was calculated to hold about 30,000 superficial feet of 1-inch
boards, which, upon the steam-pipe system, occupied full three weeks
in drying. This apparatus of Messrs. Price and Manby, with rather less
fuel, was considered to thoroughly dry each stove-full in ten days, thus
saving a consumption of ten days’ fuel, independent of the advantages
of expediting business. The average temperature was 104°, and as the
continuous stream of pure air passing between the metallic plates was
divested of its moisture, it carried off the dampness of the timber in
an imperceptible manner. An experiment was tried, by having a flooring
batten, 7 inches by 1¼ inch, cut from a piece of timber which had been
floated, and was as full of water as it could be, placed in the stove;
and when the temperature was 102°, it remained there five days, and when
sawn down into ⅝ inch thick, and planed, it was found to be perfectly dry
throughout. The heat was so gentle, and the evaporation so equal, that
the timber was never rent, as when exposed to the air and a hot sun: in
short, Messrs. Holme considered it one of the most perfect timber stoves
that had been made.

It may be remarked with respect to desiccation, that the timber to be
artificially dried is generally exposed to a great heat for a short
time, rather than to a moderate heat for a lengthened one; and the air,
saturated with the vapour thus produced, is generally very imperfectly
removed. Wood so treated is almost sure to split, from the unequal
contraction to which it is exposed; and the pores are also very liable to
reopen on the wood being withdrawn from the stove, because there is no
gradual and permanent change in their mechanical structure. It is only
within the last few years past that the artificial desiccation of wood,
before its impregnation with an antiseptic preparation in closed vessels,
has been frequently adopted in practice.

We cannot give a better termination to the few remarks we have made about
“steaming and boiling timber,” than by quoting the opinion of the late
Sir Charles Barry, R.A., architect to the new Houses of Parliament, which
we propose doing in the following manner:

“YORK ROAD, LAMBETH, _Nov. 30, 1844_.

SIR,

In reply to your application, we beg to acquaint you that we
are willing to undertake the ordinary works required in the
finishings of the new Palace of Westminster. … The wainscot to
be used in the joiner’s work is assumed to be from the best
Crown Riga wainscot in the logs, and from pipe-staves of the
best quality, in equal proportions, to be _prepared for use by
steaming_, or otherwise.…

_Grissell & Peto._”

Charles Barry, Esq.

Sir Charles Barry recommended this tender to the Treasury for acceptance;
but we fancy that he was doubtful about the efficacy of steaming, as we
think will appear from the following extract from an “Agreement between
Sir Charles Barry and Messrs. Grissell and Peto, builders:

“_First._ That the wainscot is assumed to be from the log and pipe-staves
in equal quantities; the prime cost of which, in inch boards, _seasoned
by steam_, or other artificial means, so as to be fit for use, is
calculated at 6½_d._ per foot superficial.

“_Secondly._ That _if it should be found necessary to make use of
thoroughly dry wainscot boards_ for the whole or any portion of
the joiner’s work, seasoned by natural means (viz. exposure to the
atmosphere), the prime cost of such boards, with the addition of a
profit of 7½ per cent., is to be allowed for them, over and above the
price of 6½_d._ per foot superficial, the prime cost of wainscot boards
provided for in the contract, as above stated.” (Italics are our own.)

SEASONING BY SMOKE DRYING.

Smoke drying in an open chamber, or the burning of furze, fern, shavings,
or straw under the wood, is said to give it hardness and durability;
and, by rendering it bitter, destroys and prevents worms. It also
destroys the germ of any fungus which may have commenced. It is an old
and well-founded observation that smoke drying contributes much to the
hardness and durability of woods. Virgil appears to have been aware of
its utility, when he wrote the passage which is thus translated by Dryden:

“Of beech, the plough-tail, and the bending yoke,
Or softer linden, hardened in the smoke.”--GEORGICS, i., 225.

Beckman, in his ‘History of Inventions,’ quotes a passage from Hesiod to
the same effect; and adds, “as the houses of the ancients were so smoky,
it may be easily comprehended how, by means of smoke, they could dry and
harden pieces of timber.” In this manner were prepared the pieces of wood
destined for ploughs, waggons, and the rudders of vessels:

“These long suspend, where smoke their strength explores,
And seasons into use, and binds their pores.”--VIRGIL.

The late Brigadier-General Sir Samuel Bentham bestowed much time and
attention in endeavouring to ascertain the quickest and best means of
drying oak. In his letter to the Navy Board, 6th March, 1812, he says:
“By exposing block shells to the smoke of burning wood, they become in
the course of two or three days well seasoned in every respect, hard,
bright coloured, and, as it were, polished. But it was found in a very
short time that the acid with which the shells were thus impregnated very
rapidly corroded the iron pins which passed through them.

“In Russia many small articles, such as parts of wheels, wheel carriages,
and sledges, are prepared in this manner; so are wheels, at least in some
parts of America; and sabots and other small articles in France.”

In speaking of artificial heat, he says, in the same letter:

“From all the opportunities I have had of examining the state of timber
so prepared by artificial heat, the due seasoning without cracking has
appeared to depend on the ventilation happening to be _constant_, but
very _slow_, joined to such a due regulation of the heat as that the
_interior_ of the timber should dry, and keep pace in its contraction
with the outer circles.”

Mr. T. W. Silloway, in ‘American Carpentry,’ remarks: “If timber be dried
by heat, the outside will become hardened, and the pores closed, so that
moisture, instead of passing out, will be retained within.”

Bowden remarks, “that the timbers of a small ship underwent the process
of charring, either by suspending them over a fire of chips, or by
burning the exterior with red-hot irons, so as to char the external
surface. Air trunks were also formed between the timbers, for the
purpose of evaporating moisture. The state of this vessel was examined
five years after she was launched, and it appeared that, although the
timbers had been very strongly charred, fungi had grown to a considerable
extent on both sides abaft the fore channels, and that the plank near the
magazine was completely decayed.” _The power of vegetation broke through
the incrusted barrier against external affection._

A method is in operation at Tourlaville, near Cherbourg, for which the
inventor, M. Guibert, has taken out a patent, and it is said to give at
once more expeditious and sure results than those obtained from the use
of dry and hot air. It consists in filling the drying-stove with smoke,
produced by the distillation of certain combustible matters, such as
sawdust, waste tan, and smiths’ coals, &c. By means of a ventilator,
ingeniously arranged, a rotatory movement round the logs laid to season
is given to the smoke, so as to obtain an average uniform temperature in
every part. By this plan, as the distillation of combustibles is always
attended with a considerable discharge of steam, all cracks and splits
are said to be prevented.

There is much force in Sir Samuel Bentham’s observations respecting the
drying of timber by artificial heat: it is certainly not well to attempt
to dry it _too_ quickly, for if it be subjected to great heat, a large
portion of the carbon will pass off, and thereby weaken the timber.
Timber too suddenly dried cracks badly, and is thus materially injured:
planks of larch or beech are liable to warp and twist if their drying is
hastened.

STOVE DRYING.

In some of the large manufactories for cabinet work, the premises are
heated by steam pipes, in which case they have a close stove in every
workshop heated many degrees beyond the general temperature, for giving
the final seasoning to the wood; for heating the cauls; and for warming
the glue, which is then done by opening a small steam pipe into the outer
vessel of the glue-pot. The arrangement is extremely clean, safe from
fire, and the degree of heat is very much under control.

In some manufactories, the wood is placed for a few days before it is
worked up in a drying-room heated by means of stoves, steam or hot water,
to several degrees beyond the temperature to which the finished work
is likely to be subjected. Such rooms are frequently made as air-tight
as possible, which appears to be a mistake,[1] as the wood is then
surrounded by a warm but stagnant atmosphere, which retains whatever
moisture it may have evaporated from the wood.

Fire-stoves for drying the timber were placed in the magazine,
bread-room, and other parts of the ‘Royal Charlotte’ ship; and the evil
of this practice was soon shown, for the vessel became dry rotten in
_twelve months_.[2]

Wood sometimes undergoes a baking process for veneering. Fourcroy has
recommended baking timber in an oven, and he has asserted that it would
render timber more durable; “but,” says Boyden, “it should be subjected
to a very strong heat, lest in endeavouring to prevent vegetation,
we should give it birth.” Captain Shaw[3] observes: “Any artificial
heating which burns the air is most injurious to wood and all combustible
materials, and renders them much more inflammable than they would be if
only exposed to the temperature of the atmosphere.”

SEASONING BY SCORCHING AND CHARRING.

Scorching and charring are good for preventing and destroying infection
in timber, but have to be done slowly, and only to timber that is
already thoroughly seasoned; otherwise, by incrusting the surface,
the evaporation of any internal moisture is intercepted, and decay in
the heart soon ensues; if done hastily, cracks are also caused on the
surface, and which, receiving from the wood a moisture for which there is
not a sufficient means of evaporation, renders it soon liable to decay.
Charring has little or no control over internal corruption, though it is
a good preventive against external infection: it increases the durability
of dry, but promotes the decay of wet timber. Farmers very often resort
to this method for the preservation of their fence-posts; the charring
should extend a little above their contact with the ground. Unless they
discriminate between green and unseasoned timber, these operations will
prove injurious instead of beneficial.

We have already quoted Sir Charles Barry in favour of _steaming_ wood;
we now intend giving the opinion of a former pupil of his with regard to
_charring_ it. Mr. George Vulliamy, architect to the Metropolitan Board
of Works, in a specification for oak fencing which was fixed round the
boundaries of Finsbury Park, London, in 1867, writes as follows:--“Dig
out the ground for the upright standards where shall be directed, and
fill in and ram round same with dry burnt earth, stones, and rubbish (the
burnt clay will be provided); enclose the boundaries of Park, as shall be
directed, with _dry and well-seasoned_ heart of English oak, _wrought_
upright standards, 6 inches by 5 inches, and 8 feet 6 inches total
length, with cut and _splayed_ tops, holes drilled for oak pins, and
mortised for horizontal rails, as shown on detailed drawings; to stand 5
feet 3 inches out of ground, and _the ends in ground to be well charred
before fixing_.” (The italics are our own.)

Our ancestors used charcoal and charred wood, on account of their
durability, for landmarks in the ground between estates. The
incorruptibility of charcoal is well known. Amongst other advantages,
rats will not touch it; neither will the white ants nor cockroaches, so
common in the Indies, commit their depredations where charring has been
employed.

The ‘Revue Horticole’ states that it has been proved by recent
experiments, that the best mode of prolonging the duration of wood is to
char it, and then paint it over with three or four coats of pitch. Many
of the sleepers now laid down on the Belgian railways are charred, the
engineers preferring this process to any other.

The superficial carbonization, or charring of wood, as a preservative
means, has long been practised. The Venetians have used charring for
timber for a long period, particularly for piles. In France, M. de
Lapparent recently proposed to apply it to the timber used in the French
Navy. Some experiments, which were undertaken with a view to determine
its practicability, terminated satisfactorily; and the Minister of Marine
ordered the process to be introduced into the Imperial dockyards.

M. de Lapparent makes use of a gas blowpipe, the flame from which is
allowed to play upon every part of the piece of timber in succession.
By this means the degree of torrefaction may be regulated at will. The
method is applicable to woodwork of all kinds; and the charring, it is
said, does not destroy the sharpness of any mouldings with which the wood
may be ornamented.

In the ‘Journal des Savants,’ Feb. 15, 1666, appears the following: “The
Portugals scorch their ships, insomuch that in the quick works there is a
coaly crust of about an inch thick; but this is dangerous, it happening,
not seldom, that the whole vessel is burnt.” It is no wonder that the
Portuguese ships should frequently fire in the operation, as their plank
was charred an inch deep. A mere charring, if done properly, after the
timbers had been thoroughly seasoned by air, would have been sufficient.

Charring seasoned wood is known to be a most effectual mode of
preservation against rot in timber: thus do piles, when charred, last for
ages in water or moist soil. Charred wood has been dug up, which must
have lain in the ground for 1500 years, and was then found perfectly
sound. After the Temple of Diana, at Ephesus, was destroyed, it was
found to have been built on charred piles; and at Herculaneum, after 2000
years, the charred wood was found to be whole and undiminished. But we
find Sir Christopher Wren did not approve of charred piles, except in a
soil where they would be constantly wet. So, in order to attain a firmer
foundation for St. Paul’s Cathedral, he had the ground excavated to an
immense depth before a stone of the building was laid.

From time immemorial it has been the practice, particularly in France,
to burn the ends of the poles driven into the ground to preserve them
from decay. According to the remark of the celebrated Carlomb, we should
always take into serious consideration old and well-known customs; but in
this instance it is easy to admit the preserving effect of carbonization.
Mr. James Randall,[4] Architect, states that he “oxidated several
pieces of wood with nitric acid, and with fire,” and these processes
were attended with success. Nearly the last sentence in his work is,
“_oxidation only_ can be relied on, in all cases, as an effectual cure.”

In charring, the surface of the timber is subjected to a considerable
heat, the primary effect of which is to exhaust the sap of the epidermis,
and to dry up the fermenting principles. Here this is done by long
exposure to the air; and, in the second place, below the outside layer
completely carbonized, a scorched surface is found, that is to say,
partly distilled and impregnated with the products of that distillation,
which is creosoted; the antiseptic properties of which are well known.

When Mr. Binmer was examined before the Commissioners of Woods, Forests,
&c., in 1792, he stated “that all steamed plank should be afterwards
dried and _burnt_ to extract the moisture.”

To a spontaneous carbonization must be attributed also the
unchangeableness of that timber entirely black, which is met with
everywhere in digging up the ground, where it has laid buried for ages.
In the neighbourhood of St. Malo, France, these specimens are very
common, and there most of the espaliers and vine props are made of wood,
black as ebony, and famous for its durability. They have been cut from
the trees of an old forest, submerged in the eighth century by an inroad
of the sea, which formerly crossed a Roman road, leading from Brittany to
Cotentin.

Not long after the beginning of the eighteenth century, the method of
heating or charring timber, before it was worked up, and also that of
stoving--that is, of heating in kilns with sand--were practised in
the Royal dockyards. The ‘Royal William,’ one of the most remarkable
instances of durability that the British Navy has supplied, was built
either wholly or in part of timber that had been charred. It was launched
in 1719; never repaired until 1757; and then, when surveyed afloat, in
1785, it appeared that the thick stuff and plank had been _burnt_ instead
of being _kilned_; and that the ends of the beams, the faying parts of
the breast-hooks, crutches, resters, knees, &c., had been gouged in a
manner then practised, which was called _snail-creeping_; by means of
which the air was conveyed to the different parts of the ship.[5]

The reason this method has not been persevered in, but nearly abandoned,
is owing to many causes: the difficulty and danger of the means adopted
for charring, when either straw, fern, or shavings are made use of; the
serious objection of burning the timber too deeply; or the encumbrance
of the apparatus, and the length of time occupied, if sand-kilns
sufficiently heated are used; and, finally, to indifference, or that
system of routine, against which the wisest plans often contend in vain.

In house-building, the charring process should be applied to the beams
and joists embedded in the walls, or surrounded with plaster; to the
joists of stables, washhouses, &c., which, although exposed to the free
air, are constantly surrounded by a warm and moist atmosphere, an active
cause of fermentation; to the wainscotting of ground floors; to the
flooring beneath parquet work; to the joints of tongues and rabbets;
for carbonization by means of gas still leaves to the wood, for working
purposes, all the sharpness of its edges. Charring is particularly useful
in the junction of all broad surfaces, and more essentially in those
which are cut either transverse or oblique to the grain of the wood,
as the sap vessels are then exposed to the absorption of moisture. The
butts of timbers are peculiarly liable to rot, because of affording a
lodgment for moisture without a free passage for air. No seasoned timber
should have its tubular parts exposed, nor should any timber have the saw
marks upon it, because the torn filaments absorb and retain moisture.
Allusion has already been made to the process adopted, near Cherbourg,
for preventing the decay of timber by means of gas.

By carbonization, a practical and economical means is afforded to railway
companies of preserving, almost for ever, the sleepers, and particularly
oak, which cannot be impregnated easily by the injection of mineral
salts. Let us suppose, for instance, that after, say ten or fifteen
years, the sleepers on a line are taken up for the length of a mile,
and replaced by new ones; the old, when rasped and burnt again, will
serve for the replacing the following mile, and so on, one mile after
the other. It might be equally serviceable to apply the same process to
injected beech, for the reason that it is almost impossible to make the
preserving liquid penetrate thoroughly the mass of the timber.

SEASONING BY EXTRACTION OF SAP.

Mr. John Stephen Langton’s method of seasoning by extraction of the
sap was patented in 1825, but is now almost wholly discontinued. It
consists in letting the timber into vertical iron cylinders, standing in
a cistern of water, closing the cylinders at top; and the water being
heated, and steam used to produce a partial vacuum, the sap relieved
from the atmospheric pressure oozes from the wood, and being converted
into vapour, passes off through a pipe provided for the purpose. The
time required is about ten weeks, and the cost is about ten shillings
per load; but the sap is wholly extracted, and the timber is said to
be fit and ready for any purpose; the diminution of weight is, with a
little more shrinkage, similar to that in seasoning by the common natural
process.[6]

Mr. Barlow’s patent provided for exhausting the air from one end of
the log while one or more atmospheres press upon the other end. This
artificial aerial circulation through the wood is prolonged at pleasure.
However excellent in theory, this process is not practicable.

In October, 1844, M. Tissier proposed to place wood in a close vessel,
and subject it to a current of hot dry air; and in 1847, Mr. Miller
proposed to inject hot air through beams of wood to drive out the sap.

In 1851, M. Meyer d’Uslaw proposed to first dilate the pores of the wood
with steam, and then place it in a hermetically closed chamber, and make
a vacuum there.

The following system of preparing timber for the Navy was, not many years
since, adopted in South Russia. A full account of the practice will be
found in Oliphant’s ‘Russian Shores of the Black Sea,’ 1853. The only
name we can give it is

“‘SEASONING’ BY BRIBES.”

A certain quantity of well-seasoned oak being required, Government issues
tenders for the supply of the requisite amount. A number of contractors
submit their tenders to a board appointed for the purpose of receiving
them, who are regulated in the choice of a contractor not by the amount
of his tender, but of his bribe. The _fortunate_ individual selected
immediately sub-contracts upon a somewhat similar principle. Arranging
to be supplied with the timber for half the amount of his tender, the
sub-contractor carries on the game, and perhaps the eighth link in this
contracting chain is the man who, for an absurdly low figure, undertakes
to produce the _seasoned_ wood.

His agents in the central provinces accordingly float a quantity of
green pines and firs down the Dnieper and Bog to Nicholaeff, which are
duly handed up to the head contractor, each man pocketing the difference
between his contract and that of his neighbour. When the wood is produced
before the board appointed to inspect it, another bribe _seasons_ it; and
the Government, after paying the price of well-seasoned oak, is surprised
that the 120-gun ship, which it has been built of it, is unfit for
service in five years.

“Mark but my fall, and that that ruin’d me,
Corruption.”--SHAKSPEARE.

A few words can only be given to a most important matter, viz., the
_second seasoning_, which many woods require. If floor-boards are only
laid down at first on the joists of a building, and at the expiration of
one year wedged tight and nailed down, those unsightly openings caused
by shrinkage, which form a harbour for dirt and vermin, will be avoided,
as the wood will have had an opportunity of shrinking. Doors, sashes,
architraves in long lengths, will also be better if made up some time
before they are required for use. Many Indian woods require a second
seasoning--kara mardá, for instance, a favourite wood with Indian railway
engineers. Even sál and teak are not exempt. Teak shrinks sideways least
of all woods. In the ‘Tortoise,’ store ship, when fifty years old, no
openings were found to exist between the boards; yet Colonel Lloyd says
he found the teak timbers used by him in constructing a large room in
the Mauritius to have shrunk ¾ of an inch in 38 feet. Thus a space of ⅜
of an inch must have been left at each end of the beam, where moisture
could lodge and fungi exist, obtaining their nourishment from the wood.
If unseasoned teak is used for ships, dry rot will in time find a place.
It may be said that teak is a very hard wood, and very durable; yet “the
mills of the gods,” says an ancient philosopher, “grind slow, very slow,
but they grind to powder;” _and so do the fungi mills_.

CHAPTER V.

ON SEASONING TIMBER BY PATENT PROCESSES, ETC.

Long years of practical experience has shown that timber, however prone
to dry or wet rot, may be preserved from both by the use of certain
metallic solutions, or other suitable protective matters.

All the various processes may be said somewhat to reduce the transverse
strength of the timber when dry, and the metallic salts are affected
at the iron bolts or fastenings. The natural juices of some woods do
this; and bolts which have united beams of elm and pitch pine will often
corrode entirely away at the junction.

The processes adopted for resisting the chemical changes in the tissues
of the wood are all founded on the principle that it is essential to
inject some material which shall at once precipitate the coaguable
portion of the albumen retained in the tissues of the wood in a
permanent insoluble form, so that it will not hereafter be susceptible
of putrefactive decomposition. For this purpose, many substances, many
solutions, have been employed with variable success, but materials have
been sometimes introduced for this purpose which produced an effect just
the opposite to what was anticipated.

Experience has shown that timber is permeable, at least by aqueous
solutions, only so long as the sap channels are free from incrustation.

Such in general is the case with beech, elm, poplar, and hornbeam, the
capillary tubes of which are always open, or, at least, close very
slowly. At the same time it may be said that there must remain ever in
these species some parts impervious to injection, whilst it is almost
impossible but that a certain portion of the fibres will be more or less
incrusted. The sap woods, on the other hand, of every species appear
quite pervious.

Very little is known of any preservative process adopted in ancient
times. Pliny observes that the ancients used garlic boiled in vinegar
with considerable success, especially with reference to preserving timber
from worms: he also states that the oil of cedar will protect any timber
anointed with it from worm and rottenness. Oil of cedar was used by the
ancient Egyptians for preserving their mummies. Tar and linseed oil were
also recommended by him. The image of the goddess Diana, at Ephesus,
was saturated with olive and cedar oils; also the image of Jupiter, at
Rome; and the statues of Minerva and Bacchus were impregnated with oil of
spikenard.

The idea of preserving wood by the action of oil is therefore by no means
new; but it is somewhat curious that the earliest modern processes should
also be by means of oil. The _oils most proper_ to be used are _linseed_,
_rapeseed_, or almost any of the vegetable fixed oils. Oak wood, rendered
entirely free from moisture, and then immersed in linseed oil, is said
to be thus prevented from splitting: the time of immersion depending on
the size, &c. Palm oil is preferable to whale oil, because impregnation
with the latter, although in many instances eligible, causes wood to
become brittle. It is, however, probable that whale oil, when combined
with other substances, such as litharge, coal pitch, or charcoal,
may lose much of that effect. As cocoa-nut oil, which is, under low
temperature, like the oil expressed from the nuts of the palm tree, is
known to be highly preservative of timber and metallic fastenings, we may
expect the same result from the latter, and thereby avoid that extreme
dryness and brittleness of the timber which Mr. Strange complained of
in the Venetian ships that had been seasoned for many years in frame
under cover. Cocoa-nut oil beat up with shell lime or _chunam_, so as to
become putty, and afterwards diluted with more oil, is used at Bombay and
elsewhere as a preservative coat or varnish to plank. It cannot become
a varnish without the addition of some essential oil; and the oil of
mustard is used; which, of course, will produce the desired effect. In
the first volume of the Abbé Raynal, on the European settlements in the
East and West Indies, he mentions that an oil was exported from Pegu for
the preservation of ships; but as he does not say what oil, no conclusion
can be drawn further than as to the probability of its being one of those
already noticed.

Experience has proved that even _animal oils_ are so far injurious
to timber as to _render it brittle_, whilst they preserve it from
rottenness; and that, on the other hand, a mineral salt more or less
combined with fatty substances does not produce that effect. The staves
of whale-oil casks become quite brittle, whilst those of beef, pork,
and tallow barrels remain tough and sound. Ships _constantly_ in the
Greenland trade have their timbers and planks preserved so far as they
have become impregnated with whale oil.

Experiments with fish oil prove that of itself, unless exposed to sun and
air, it may be injurious; that it loosens the cohesion of timber; but
that _animal fat_, combined _with saline matter_, _is preservative_.

Fish oil used alone is ineligible, because capable of running into the
putrefactive process, unless as a thin outside varnish. In hard, sound
timber, it will hardly enter at all; and if poured into bore-holes in the
heads of timbers, it will insinuate itself into the smallest rents or
cracks, and waste through them. Used alone, or with any admixture, it is
absorbed and dried quickly on wood in a decomposing state or commencing
to be dry rotten. Used with litharge, it dries after some days; but
with lamp-black it has scarcely so much tendency to dry as when used
alone. Paint of fish oil and charcoal dries very quickly where there is
absorption, and the charcoal extends its oxidating or drying effect to
the fish oil in its vicinity.

We give the following to prove what we have written, and also to serve as
an example for those who wish to try experiments:--

EXPERIMENTS ON FISH OIL.

June 9.--Upon a piece of old oak scantling, with its alburnam
on one side in a state of decay, fish oil was poured several
times, viz. on this day, on June 25, and July 3, which it rapidly
absorbed in the decayed part.

July 26.--It was payed (or mopped) with fish oil and charcoal
powder, and the following day it was put under an inverted cask.

October 1.--The end of this piece was covered with a greenish
mould. _This proves that fish oil must be injurious, except where
exposed to sun and air to dry it._

A compound of fixed oils and charcoal is liable to inflame, but as a thin
covering or pigment it may not be so.

The _petroleum_ oil-wells, near Prome, in Burmah, have been in use from
time immemorial. Wood, both for ship-building and house-building, is
invariably saturated or coated with the product of those wells; and
it is stated that the result is _entire immunity from decay_ and the
ravages of the white ant. At Marseilles, and some other ports in the
Mediterranean, it used to be the practice to run the petroleum, which
is obtained near the banks of the Rhone, into the vacancies between the
timbers of the vessels, to give them durability. It was sometimes, for
the conjoint purpose of giving stability and duration to vessels, mixed
with coarse sand or other extraneous matters, and run in whilst hot
between the ceiling and bottom plank, where it filled up the vacancies
between the timbers in the round of their bottoms, excepting where
necessary to be prevented. The great objection to the use of petroleum is
its inflammability. _Creosote_, its great rival for wood preserving, is
also inflammable, and not so agreeable in colour; but it is _considerably
cheaper_, which is an important matter.

As we are now about to enter upon the subject of patent processes, &c.,
it appears desirable to lay down certain principles at the commencement,
in order to assist the reader as much as possible.

Almost every chemical principle or compound of any plausibility has been
suggested in the course of the last hundred and fifty years; but the
multiplicity and contradiction of opinions form nearly an inextricable
labyrinth. To commence.

1st. It seems obvious that _the sooner the sap is wholly removed from the
wood the better_, _provided the woody fibre solidifies without injury_.

2nd. That _the wood should be impregnated with any strongly antiseptic
and non-deliquescent matter_, _which must necessarily be in solution when
it enters the wood_. No deliquescent remedy is eligible, because moisture
is injurious to metallic fastenings.

3rd. _The wood should be first dried, and its pores then closed with
any substance impervious to air and moisture, and at the same time
highly repellant to putrescency._ The most essential requisites in a
preservative of timber being a disposition to _dryness_, and a tendency
to resist _combustion_ as far as consistently obtainable.

4th. _Any process to be successful ought not to be tedious, very
difficult, or too expensive._ These are important elements in the success
of any patent.

Very little is known of any preservative process previous to the year
1717, when directions were given by the Navy authorities to _boil_
treenails, and dry them before they were used. But whether the custom had
prevailed before this time, or whether their strength and durability were
increased by it, there are no means of ascertaining. It does not appear
that any substance was put into the water to decompose the juices; but
as they are soluble in warm water, perhaps the power of vegetation might
have been destroyed without it.

In 1737 Mr. Emerson patented a process of saturating timber with _boiled
oil_, mixed with poisonous substances; but his process was very little
used. This, we believe, was the _first_ patent on wood preserving.

About 1740, Mr. Reid proposed to arrest decay by means of a certain
_vegetable acid_ (probably pyroligneous acid). The method of using it was
by simple immersion.

In 1756, Dr. Hales recommended that the planks at the water-line of ships
should be soaked in _linseed oil_, to prevent the injury to which wood
is subject when alternately exposed to wet and dry; and indeed, many
ships were built in which a hollow place was cut in one end of each beam
or sternpost, which might constantly be kept filled with _train oil_.
Amongst other ships so constructed, the ‘Fame,’ 74, may be mentioned.
When, after some years, this ship was repaired, it was found that as
far as the oil had penetrated, namely, from 12 to 18 inches from the
end, the wood was quite sound, whilst the other parts were more or less
decayed. The Americans used to hollow out the tops of their masts in the
form of cups or basins; bore holes from the end a considerable way down
the masts; pour oil into these; cover them over with lead; and leave the
oil to find its way down the capillary vessels to the interior of the
timber.[7]

In 1769, Mr. Jackson, a London chemist, with a view to the prevention
of decay, obtained permission to prepare some timber to be used in the
national yards, by immersing it in a solution of _salt water_, _lime_,
_muriate of soda_, _potash_, _salts_, &c., the result of which dose was,
that several frigates in the Navy subjected to the process were rendered
more perishable than if they had been constructed of unprepared timber.
The solution was filtered into the wood partly by means of holes made in
it. Chapman proposed a similar method of preserving the frames of ships,
viz. by boring holes in the timbers, and pumping a _solution of copperas_
in water into them. He believed every part of the vessel would thus be
impregnated.

Mr. Jackson also prepared the frame of the ship ‘Intrepid’ with another
solution. The ship lasted many years. Bowden thought it was a _solution
of glue_. Chapman suggested _slaked lime_, thinned with a weak _solution
of glue_ for mopping the timbers of a ship.

Shortly after Mr. Jackson’s process was started, Mr. Lewis attempted
to accomplish the preservation of timber by placing it surrounded by
pounded lime, in spaces below the “surface of the earth.” The use of lime
has also been advocated by Mr. Knowles, Secretary of the Committee of
Surveyors of the Navy, who has written an able work on the ‘Means to be
taken to Preserve the British Navy from Dry Rot’ (1821).

Between 1768 and 1773 a practice prevailed of saturating ships with
common salt; but this was found to cause a rapid corrosion of the iron
fastenings, and to fill the vessels between decks with a constant damp
vapour. In ‘Nicholson’s Journal,’ No. 30, there is an article signed
_Nauticus_ on this subject. Vessel owners had long ago observed that
those ships which have early sailed with cargoes of salt are not attacked
by dry rot. Indeed, several instances are attested of vessels whose
interiors were lined with fungi having all traces of the plant destroyed
by accidental or intentional sinking in the sea. Acting on such hints,
a trader of Boston, U. S., salted his ships with 500 bushels of the
chloride, disposed as an interior lining, adding 100 bushels at the end
of two years. Such an addition of dead weight is sufficient objection to
a procedure which has other great disadvantages. Salt should never be
applied as an antidote against the dry rot, on account of its natural
powers of attracting moisture from the atmosphere, which would render
apartments almost uninhabitable, from their continual dampness. Those who
have lived for any length of time in a house at the sea-side, the mortar
of which has been partly composed of sea sand, will have observed the
moist state of the paper, plastering, &c., in wet weather. Bricks made
with sea sand are objectionable.

_Salt water_ seasoning has already been referred to in the last chapter,
but as it is so closely connected with salt seasoning, the further and
final consideration of salt water seasoning may be fitly dealt with
here. Salt water will not extract the juices from the timber like fresh
water. It is only by destroying the vegetation that salt water can be
advantageous, but it would require a very long time to impregnate large
timber to the heart so as to destroy vegetation. It is well known that
wood is softened, and in time decomposed, by extreme moisture. Fifty
years since, the master builder at Cronstadt complained that the oak from
Casan, which was frequently wet from different causes in its passage of
three years to Cronstadt, was so water-soaked as never to dry; and also
from the information of Mr. Strange, it appears “that the practice at
Venice of the fresh-cut timber being thrown into salt water, prevents
its ever becoming dry in the ships, and that the salt water rusted and
corroded the iron bolts.” In fine, vessels built with salt water seasoned
wood are perfect hygrometers, being as sensible to the changes of the
moisture of the atmosphere as lumps of rock salt, or the plaster of
inside walls where sea sand has been used.

In Ceylon, the timber of the female palm tree is much harder and blacker
than that of the male, inasmuch as it brings nearly triple its price.
The natives are so well aware of the difference that they resort to the
devise of immersing the male tree in _salt water_ to deepen its colour,
as well as add to its weight.

Vessels impregnated with _bay salt_, or the large grained salt of
Leamington or of Liverpool (pure muriate of soda), will possess decided
advantages; as also will vessels that have been laden with _saltpetre_,
if it has been dispersed amongst their timbers.

Ships (the timbers of which had been previously immersed in salt water)
have been broken up after a few years’ service, and the floor timbers
taken out quite sound: but when exposed to the sun and rain in the summer
months, their albumen has been in a decomposed or friable state.

By the answers to queries given to Mr. Strange, the British Minister at
Venice, in or about 1792, it appears that several of the Venetian ships
of war had then lain under sheds for fifty-nine years; some in bare
frames, and others planked and caulked: that these ships show no outward
marks of decay; but their timbers have shrunk much, and _become brittle_;
that some of the most intelligent ship builders were of opinion that
great prejudice had arisen from the prevalent custom of throwing the
timber fresh cut into salt water, and letting it lie there until wanted;
that afterwards it dried, and withered on the outside, under the sheds,
while the inside, being soaked with salt water, rotted before it became
dry; and this was one reason, amongst others, why Venetian ships, though
built of good timber, lasted so short a time; for the salt moisture not
only rots the inside of the beams and timbers, but of course rusts and
corrodes the iron bolts.

_Salt water_, _sea-sand_, and _sea-weed_ are now used for seasoning
“jarrah” wood in Western Australia. This wood is considered a first-class
wood for ship-building, but it is somewhat slow to season, and if exposed
before being seasoned it is apt to “fly” and cast. The method adopted
is as follows: The logs are thrown into the sea, and left there for a
few weeks; they are then drawn up through the sand, and after being
covered with sea-weed a few inches deep, are left to lie on the beach,
care being taken to prevent the sun getting at their ends. The logs are
then left for many months to season. When taken up they are cut into
boards 7 inches wide, and stacked, so as to admit of a free circulation
of air round them, for five or six months before using them. Sea-weed or
sea-ware, cast upon the shores, contains a small quantity of carbonate
of soda, and a large proportion of nitrogenous and saline matters, with
earthy salts, in a readily decomposable state. They also contain much
soluble mucilage. The practice of seasoning timber by heating it in a
_sand bath_ was formerly adopted by the Dutch, and by the Russians in
building boats. Mr. Thomas Nichols (in a letter to Lord Chatham, when
First Lord of the Admiralty) states “that the same end, viz. preservation
of timber from decay, might probably be acquired by burying the timber in
sand, which acts as an artificial sap,” in the same manner as mentioned
in Townsend’s ‘Travels through Spain,’ to be used with the masts of ships
of war at Cadiz.

_Peat moss_ has been recommended (because the sulphates of iron, soda,
and magnesia are found in it), but it failed when tried.

With reference to Mr. Lewis’s proposal to preserve wood by means of
lime, it must be remembered that _quicklime_, with damp, has been found
to accelerate putrefaction, in consequence of its extracting carbon;
but when dry, and in such large quantities as to absorb all moisture
from the wood, _the wood is preserved_, _and the sap hardened_. Vessels
_long_ in the lime trade have afforded proof of this fact; and we have
also examples in plastering-laths, which are generally found sound and
good in places where they have been dry. Whitewash or _limewater_ has
been strongly recommended for use between the decks of ships, as being
unfavourable to vegetation: it should be renewed at intervals of time,
according to circumstances. It has been applied with good effect to the
joists and sleepers of kitchen floors; but to be effectual it should be
occasionally renewed. Effete, or re-carbonated lime, is injurious to
timber, like other absorbent earths; so also are calcareous incrustations
formed by the solution of lime in water, as appears from Von Buch’s
‘Travels in Norway,’ in which he says, “that in the fishing country (near
Lofodden, beyond the Arctic circle) the calcareous incrustations brought
by water, filtering through a bed of shells, soon cause the vessels and
wood to be covered with and destroyed by green fungi.” The ends of joists
of timber inserted in walls are frequently found rotten; and where not
so, it may probably be owing to the mortar having been made with hot
lime, and used immediately, or to the absence of moisture. It does not
appear practicable to use limewater to any extent for preserving timber,
because water holds in solution only about ⅟500th part of lime, which
quantity would be too inconsiderable; it, however, renders timber more
durable, but at the same time very hard and difficult to be worked (p.
73).

Vessels constantly in the _coal_ trade have generally required little
repair, and have lasted until in the common course of things they were
lost by shipwreck. This must be owing to the martial pyrites which abound
in all coals; and also from the sulphuric acid arising from the quantity
of coal dust which finds its way through the seams of the ceiling, and
adheres to the timber and planks.

In 1779, M. Pallas, in Russia, proposed to steep wood in _sulphate of
iron_ (green vitriol) until it had penetrated deeply, _and_ then in
_lime_ to precipitate the vitriol. Neumann, in his first volume of
‘Chemistry,’ on the article green vitriol, says, “That in the Swedish
transactions this salt is recommended for preserving wood, particularly
the wheels of carriages, from decay.

“When all the pieces are fit for being joined together, they are directed
to be boiled in a solution of vitriol for three or four hours, and then
kept for some days in a warm place to dry. It is said that the wood
by this preparation becomes so hard and compact that moisture cannot
penetrate it, and that iron nails are not so apt to be destroyed in this
vitriolated wood as might be expected, _but last as long as the wood
itself_.”

In 1780 the marcasite termed by the miners _mundic_, found in great
abundance in the tin mines in Devonshire and Cornwall, was employed, in
a state of fusion, to eradicate present and to prevent the future growth
of dry rot; but whether its efficacy was proved by time is not known. A
garden walk where there are some pieces of mundic never has any weeds
growing; the rain that falls becomes impregnated with its qualities, and
in flowing through the walk prevents vegetation.

In 1796 Hales proposed to _creosote_ the treenails of ships: this was
forty-two years previous to Bethell’s patent for creosoting wood.

About the year 1800, the Society of Arts’ building in the Adelphi,
London, being attacked by dry rot, Dr. Higgins examined the timbers,
caused some to be removed and replaced by new, and the remainder to be
scraped and washed with a solution of _caustic ammonia_, so as by burning
the surface of the wood to prevent the growth of fungi.

At the commencement of the present century, a member of the Royal Academy
of Stockholm called attention to the use of _alum_ for preserving wood
from fire. He says, in the Memoirs of that Academy, “Having been within
these few years to visit the alum mines of Loswers, in the province of
Calmar, I took notice of some attempts made to burn the old staves of
tubs and pails that had been used for the alum works. For this purpose
they were thrown into the furnace, but those pieces of wood which had
been _penetrated_ by the alum did not burn, though they remained for
a long time in the fire, where they only became red; however, at last
they were consumed by the intenseness of the heat, but they yielded no
flame.” He concludes, from this experiment, that wood or timber for the
purpose of building may be secured against the action of fire by letting
it remain for some time in water wherein vitriol, alum, or any other salt
has been dissolved which contains no inflammable parts.

In Sir John Pringle’s Tables of the antiseptic powers of different
substances, he states _alum_ to be thirty times stronger than sea-salt;
and by the experiments of the author of the ‘Essai pour servir à
l’Histoire de la Putréfaction,’ metallic salts are much more antiseptic
than those with earthy bases.

In 1815 it occurred to Mr. Wade that it would be a good practice to fill
the pores of timber with _alumine_, or selenite; but two years after,
Chapman observed, “Impregnation of ships’ timbers with a _solution of
alum_ occurred to me about twenty years since, because on immersion in
sea-water the alumine would be deposited in the pores of the timber; but
I was soon informed of its worse than inutility, by learning that the
_experiment had been tried_, and, in place of preserving, had _caused the
wood to rot speedily_. Impregnation with _selenite_ has been tried in elm
water-pipes. On precipitation from its solvent it partially filled the
pores, and hardened the wood, but _occasioned speedy rottenness_.” If,
by using a _solution of alum_ to render wood uninflammable, we at the
same time cause it to _rot speedily_, it becomes a question _whether the
remedy is not worse than the disease_. Captain E. M. Shaw, of the London
Fire Brigade, in his work, ‘Fire Surveys’ (1872), recommends _alum and
water_. Probably he only thought of fire, and not of rotting the wood.
The alum question does not appear to be yet satisfactorily settled.

While upon the subject of uninflammable wood, we may state that in 1848,
upon Putney Heath (near London), by the roadside, stood an obelisk, to
record the success of a discovery made in the last century of the means
of building a house which no ordinary application of ignited combustibles
could be made to consume: the obelisk was erected in 1786. The inventor
was Mr. David Hartley, to whom the House of Commons voted 2500_l._, to
defray the expenses of the experimental building, which stood about one
hundred yards from the obelisk. The building was three stories high, and
two rooms on a floor. In 1774, King George the Third and Queen Charlotte
took their breakfast in one of the rooms, while in the apartment b

Read full text (200,001 characters)

Fields

authorThomas Allen Britton
languageEnglish
chars567205
source_urlhttps://www.gutenberg.org/ebooks/55541

Cite this record

MLA
"A treatise on the origin, progress, prevention, and cure of dry rot in timber." Project Gutenberg, n.d., https://gutenberg.go-v.org/record/55541.

Chicago
"A treatise on the origin, progress, prevention, and cure of dry rot in timber." Project Gutenberg. n.d.. https://gutenberg.go-v.org/record/55541.

APA
Project Gutenberg. (n.d.). A treatise on the origin, progress, prevention, and cure of dry rot in timber. https://gutenberg.go-v.org/record/55541

Share card · JSON record

source: Project Gutenberglicence: Public domain (per item)year: —id: 55541citation: https://www.gutenberg.org/ebooks/55541

JSON · full text · full-text JSON ·

Related services and records

Services

  • Estate — measured countries, lanes and facts
  • Intel — live corroborated events
  • Legal — statutes, cases and citations
  • Encyclopedia — articles with inline sources
  • Space — launches, satellites and orbits
  • Search — federated search and reports
  • Pass — passport account and SSO
  • Corpora — read-only corpus origins
  • e01 — self-hosted corpora and tools

Text and metadata only; each target carries its own sources. Missing data is published as no-data, never estimated.