Modern Copper Smelting
The Project Gutenberg eBook of Modern Copper Smelting This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Modern Copper Smelting Author: Donald M. Levy Release date: October 23, 2019 [eBook #59328] Language: English Other information and formats: www.gutenberg.org/ebooks/59328 Credits: Produced by deaurider, Paul Marshall and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) *** START OF THE PROJECT GUTENBERG EBOOK MODERN COPPER SMELTING *** Produced by deaurider, Paul Marshall and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) MODERN COPPER SMELTING. _The Colour of the Converter Flame during the Bessemerising of Copper Matte._ [Illustration: FIG. 1. Flame at commencement of blow.] [Illustration: FIG. 2. Flame during the first or “slagging” stage.] [Illustration: FIG. 3. “White Metal stage.” Slagging of Copper.] [Illustration: FIG. 4. Flame during second or “blowing to blister” stage.]
The Project Gutenberg eBook of Modern Copper Smelting
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: Modern Copper Smelting
Author: Donald M. Levy
Release date: October 23, 2019 [eBook #59328]
Language: English
Other information and formats: www.gutenberg.org/ebooks/59328
Credits: Produced by deaurider, Paul Marshall and the Online
Distributed Proofreading Team at http://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)
*** START OF THE PROJECT GUTENBERG EBOOK MODERN COPPER SMELTING ***
Produced by deaurider, Paul Marshall and the Online
Distributed Proofreading Team at http://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)
MODERN COPPER SMELTING.
_The Colour of the Converter Flame during the Bessemerising of Copper
Matte._
[Illustration: FIG. 1. Flame at commencement of blow.]
[Illustration: FIG. 2. Flame during the first or “slagging” stage.]
[Illustration: FIG. 3. “White Metal stage.” Slagging of Copper.]
[Illustration: FIG. 4. Flame during second or “blowing to blister”
stage.]
MODERN COPPER SMELTING.
BEING
_LECTURES DELIVERED AT BIRMINGHAM UNIVERSITY
GREATLY EXTENDED AND ADAPTED, AND WITH
AN INTRODUCTION ON THE HISTORY, USES
AND PROPERTIES OF COPPER._
BY
DONALD M. LEVY, M.Sc., Assoc. R.S.M.,
ASSISTANT LECTURER IN METALLURGY,
UNIVERSITY OF BIRMINGHAM.
With frontispiece, and 76 illustrations.
[Illustration]
LONDON:
CHARLES GRIFFIN & COMPANY, LIMITED;
EXETER STREET, STRAND.
1912.
[_All Rights Reserved._]
PREFACE.
The lectures on “Modern Copper Smelting” embodied in this volume were
delivered at the University of Birmingham to the Senior Students in the
School of Metallurgy and to others interested in the subject.
They are based largely upon the results of a study of the practice as
conducted at a number of the best organised smelters and refineries
in the United States of America, at which the author has had the
opportunity of spending some considerable time, and it has been felt
that there exists a scope, particularly on this side of the Atlantic,
for a compact volume dealing broadly with the principles underlying
Modern Copper Smelting, illustrated with such examples of working
practice from personal observation. The subject-matter of the Lectures
has been extended by the addition of an Introduction on the History,
Uses, and General Metallurgy of Copper as applied to Modern Practice.
The Copper Industry is already fortunate in the literature at its
disposal. It possesses standard works of reference through the
publication of Dr. Peters’ classical volumes on the _Principles of
Copper Smelting_, and more recently (during the preparation of the
present work) of the volume on the _Practice of Copper Smelting_—works
which have done much to raise copper smelting to a science. The
industry is being rendered invaluable service by the Technical
Societies and Technical Press, whose publications furnish an admirable
record of the constant advance in the theory and practice of the art.
Use has been made of these sources of information in the present work,
and lists of such references are appended to each of the Lectures.
Grateful acknowledgment is made to several authors and editors who have
given permission for the reproduction of illustrations or for the
inclusion of references:—Dr. Peters, Professor Gowland, Mr. Hughes, the
Editors of the _Engineering and Mining Journal_, _Mineral Industry_,
_Mines and Minerals_, and others. The Institution of Mining and
Metallurgy, Messrs. Chambers Bros., The Traylor Engineering Co., and
the Power and Mining Machinery Co. have very kindly provided blocks for
several of the illustrations; the Anaconda Copper Mining Co. furnished
a set of photographs, whilst Figs. 8, 37, and 76 have been reproduced
by permission of the American Institution of Mining Engineers.
To the Superintendents and Staffs of the several smelters where
opportunities were so freely given for studying modern practice, and
particularly to Mr. E. P. Mathewson at Anaconda, Montana, to Mr. J.
Parke Channing at the Tennessee Copper Company’s Smelter, and to Mr. W.
H. Freeland at Ducktown, Tennessee, the author desires to express his
appreciation for much valued information and many other kind services.
The frequent references made in this book to the organisation and the
methods employed at these works is not only a tribute to the useful
information freely imparted, but is also due to the fact that such
features are so thoroughly representative of the most advanced practice
in copper smelting upon a large scale and of the direction in which all
modern work is undoubtedly tending.
The author further thanks Professor Turner of Birmingham University for
his interest in this volume, Mr. Frank Levy for reading the proofs, and
the publishers, Messrs. Charles Griffin & Co., Ltd., for the care taken
in the preparation and production of the work.
UNIVERSITY OF BIRMINGHAM,
_May_, 1912.
CONTENTS.
LECTURE I. PAGES
History of Copper — Development of the
Copper Industry — Progress of Smelting
Practice — Price and Cost of Production of
Copper — Copper Statistics, 1–17
LECTURE II.
The Uses of Copper: as Metal and as
Alloy — The Physical Properties of
Copper — Effects of Impurities — Mechanical
Properties — Chemical Properties, 18–34
LECTURE III.
Compounds of Copper — Copper Mattes — The
Varieties of Commercial Copper — Ores
of Copper — Preliminary Treatment of
Ores — Sampling, 35–50
LECTURE IV.
Modern Copper Smelting Practice — Preliminary
Treatment of Ores: Concentration, Briquetting,
Sintering — The Principles of Copper Smelting
— Roasting, 51–80
LECTURE V.
Reverberatory Smelting Practice: — Functions
of the Reverberatory Furnace — Requirements
for Successful Working — Principles of Modern
Reverberatory Practice — Operation of Modern
Large Furnaces — Fuels for Reverberatory Work;
Oil Fuel; Analysis of Costs — Condition of the
Charge, 81–112
LECTURE VI.
Blast-Furnace Practice: — Functions of the
Furnace — Reduction Smelting — Oxidation
in the Furnace — The Pyritic Principle
— Features of Modern Working: Water-Jacketing,
Increase in Furnace Size, External Settling
— Constructional Details of the Furnace, 113–145
LECTURE VII.
Modern Blast-Furnace Practice
(_continued_): — Charge Calculations
— Working — Disposal of Products — Pyritic
Smelting — Sulphuric Acid Manufacture from
Smelter Gases, 146–191
LECTURE VIII.
The Bessemerising of Copper
Mattes: — Development of the Process — The
Converter — Converter Linings — Grade of
Matte — Operation of the Process — Systems
of Working, 192–216
LECTURE IX.
The Purification and Refining of Crude
Copper: — Preliminary Refining and
Casting into Anodes — Electrolytic
Refining — Bringing to Pitch, and Casting
of Merchant Copper, 217–243
INDEX, 245–259
LIST OF ILLUSTRATIONS.
FRONTISPIECE—The Colour of the Converter Flame during
the Bessemerising of Copper Matte.
PAGE
Fig. 1.—Fluctuations in the Price of Best Select Copper, 12
" 2.—Annual Production of Copper, 16
" 3.—Equilibrium Diagram, Cu-Zn Series, 22
" 4.—Influence of Arsenic and Antimony on the
Electrical Conductivity of Copper, 25
" 5.—Relations of Copper and Oxygen, 27
" 6.—Microstructure of Copper containing Oxygen
(Heyn), _Plate to face_ 28
" 7.—Relations of Copper and Arsenic, 29
" 8.—Freezing-Point Curve of Iron-Copper Sulphides
(Mattes), 38
" 9.—Outline of Sampling Scheme, Anaconda, 48
" 10.—Section through Sampling Mill, 48
" 11.—Brunton Sampler, 49
" 12.—Outline of Smelting Scheme at the Anaconda
Smelter, Montana, U. S. A., 54
" 13.—Sketch Plan of Briquetting Plant, 56
" 14.—Section through Auger-Former, showing
Briquetting Mechanism of Chambers’ Machine, 56
" 15.—Chambers’ Briquette-making Machine,
_Plate to face_ 57
" 16.—Dwight-Lloyd Sintering Machine, 60
" 17.—O’Harra Furnace (Fraser-Chalmers), illustrating
Principle of Mechanical Rabbling by Travelling
Ploughs, 71
" 18.—Section through Mechanically Rabbled Roaster
Furnace (illustrating Improvements for Protecting
Driving Mechanism), 71
" 19.—MacDougal Roaster—Vertical Section, 74
" 20.—Herreshof Furnace—Section indicating
Connections for Cooling Rabbles and Spindles, 74
" 21.—Spindle Connections and Guide Shields of
Evans-Klepetko Roasters, 76
" 22.—Rabble-blades and Bases, 77
" 23.—Development of the Reverberatory Furnace
(Gowland), 90
" 24.—Draft Pressure Record of Anaconda Reverberatory
Furnace, 94
" 25.—Skimming Reverberatory Furnace, Anaconda,
_Plate to face_ 96
" 26.—Transverse Section of Modern Reverberatory
Furnace, Anaconda, indicating Foundations,
Hearth, and Bracing, 96
" 27.—Reverberatory Furnace under Construction,
_Plate to face_ 96
" 28.—Sectional Plan and Elevation of Reverberatory
Furnace at Anaconda, 98
" 29.—Fire-box End of Reverberatory Furnace, showing
massive Bracing, Charge Bins, and Charging Levers,
Anaconda, _Plate to face_ 100
" 30.—Interior of Reverberatory Furnace (looking
towards Skimming Door), showing Expansion Spaces
in Roof, and Charging Holes, Anaconda,
_Plate to face_ 100
" 31.—Shelby Oil-Burner for Reverberatory Furnace Use, 106
" 32.—Modern Blast-Furnace Shell of Sectioned Jackets
(P. & M. M. Co.), _Plate to face_ 122
" 33.—Blast-Furnaces under Construction, showing
Fixing of Jackets, Bottom Plate, Method of
Support, Sectioning, etc. (T. E. Co.),
_Plate to face_ 124
" 34.—Development of the Blast Furnace (Gowland), 126
" 35.—Plan of 51-foot Blast Furnace, Anaconda,
indicating Position of Crucibles, Spouts, and
Connecting Bridge between Old Furnaces, 128
" 36.—Longitudinal Section and Part Elevation of
87-foot Blast-Furnace, Anaconda, indicating
Crucibles of Old Furnaces, Bridge, and Jacketing, 128
" 37.—Copper Contents in the Slags accompanying Mattes
of Various Grades, 132
" 38.—Water-Jacketed Blast Furnace, lower portion
indicating Air and Water Connections, Bottom
Supports, End Slag Spouts, etc.
(P. & M. M. Co.), _Plate to face_ 134
" 39.—Tapping Breast of Blast Furnace, Cananea, 136
" 40.—Rivetted Steel Water-Jacket, showing Tuyere
Holes and Water Inlets, etc. (P. & M. M. Co.), 137
" 41.—Transverse Section through Modern Blast Furnace,
showing Arrangements of Boshed Lower Jackets,
Upper Jackets, and Plates, Stays and Supports,
etc., 138
" 42.—Interior of Anaconda Blast Furnace, showing
Jacketing, Tuyere Holes, and Bridge,
_Plate to face_ 138
" 43.—Showing Upper Jackets, Apron and Mantle Plates
and Superstructure of Blast Furnace, Anaconda,
_Plate to face_ 140
" 44.—Charging Blast Furnaces, Anaconda,
_Plate to face_ 140
" 45.—Blast-Furnace Shell, with Air Connections
(P. & M. M. Co.), 142
" 46.—Details of Tuyere, Cananea Blast Furnace, 142
" 47.—=V=-Shaped Charging Car, indicating Mechanism
for Release and Tilting, 153
" 48.—End View of Blast Furnace, showing Tilting of
Charge Car, Anaconda, 155
" 49.—Hodge’s Charging Car, 155
" 50.—Freeland Charging Machine (D. S. C. & I. Co.), 157
" 51.—Freeland Charger-Details, 157
" 52.—Slag Spout, showing Method of Trapping Blast,
also Replaceable Nose-Piece of Spout (A), 159
" 53.—Details of Slag Spout, Cananea, 161
" 54.—Slag Spout, showing Method of Support, 161
" 55.—General View of Settler (T. E. Co.), 163
" 56.—Method of Lining Settler, Cananea, 163
" 57.—Arrangement for Matte and Slag Discharge from
Settlers (T. C. C.), 164
" 58.—Tap-hole Casting and Detail for Settlers, 165
" 59.—Anaconda Blast Furnace (51 feet long), showing
Settlers, _Plate to face_ 166
" 60.—Hoppers of Flue-Dust Chambers and Tracks for
Cars underneath, 167
" 61.—Slotted Tuyeres, 12 inches by 4 inches
(T. C. C.), 185
" 62.—Sectional Elevation and Plan of Barrel-Shaped
Silica-Lined Converter (Peters), 196
" 63.—Latest Form of Silica-Lined Barrel Converter, 197
" 64.—Longitudinal Section of Basic-Lined Converter, 198
" 65.—Basic-Lined Converter, indicating Tuyeres,
Lining, &c., 199
" 66.—Composition of a Charge during Bessemerising
Operation, 208
" 67.—Pouring Slag, Anaconda, 209
" 68.—General View of Converter Shop, Anaconda,
_Plate to face_ 214
" 69.—Sectional Plan, Elevation, and Transverse
Sections of Refining and Anode-Casting Furnace,
Anaconda (Peters), 220
" 70.—Indicating Tilting and Pouring Mechanism of
Ladle of Casting and Refining Furnaces, 225
" 71.—Walker’s Anode-Casting Machine,
_Plate to face_ 226
" 72.—General View of Tank-room of Electrolytic
Refinery (Perth Amboy, N.J.),
_Plate to face_ 226
" 73.—Indicating Methods of Suspending and Connecting
Electrodes (Perth Amboy, N.J.), 234
" 74.—Indicating Connections for Circulation of
Electrolyte (Barnett), 235
" 75.—Tank-house, showing Anode Crane (Ulke), 237
" 76.—Microstructure of Commercial Copper containing
Oxygen (Hofman), _Plate to face_ 242
TABLES.
TABLE PAGE
I. The Production of Copper, 15
II. North American Production of Copper, 17
III. Influence of Impurities on the Electrical Conductivity
of Copper, 23
IV. Analysis of Various Commercial Coppers, 44
V. Development in Size of the Reverberatory Furnace, 89
VI. Daily Reports. Reverberatory Furnaces, 102
VII. Daily Assay Report. Reverberatory Furnaces, 103
VIII. Monthly Report. Reverberatory Furnaces, 104
IX. Effect on Coke Consumption of Increased Sulphur in
the Furnace Charge, 120
X. Blast-Furnace Charge Calculations, 151
XI. Typical Charging Tables at Pyritic Smelter, 187
XII. Changes in Composition during Bessemerising, 206
COPPER SMELTING.
LECTURE I.
History of Copper — Development of the Copper
Industry — Progress of Smelting Practice — Price and
Cost of Production of Copper — Copper Statistics.
=The History of Copper.=—Copper was probably the earliest metal
commonly employed by mankind. It occurs in the native condition in
various parts of the world, and the natural product thus required no
metallurgical treatment prior to use. Its malleability and the property
of being readily toughened by simple mechanical treatment were also
factors which account for the discovery of its general usefulness in
such primitive times.
Although silver and gold were possibly known even earlier, these metals
appear to have been employed chiefly for ornamental purposes, and as
tokens, rather than for general service.
The alloy of copper and tin, known as bronze, was the first metallic
combination in common use by man; its employment was so characteristic
in prehistoric times, that archæologists assign to one of the epochs
the name of the Bronze Age. As is well known, archæological time is
marked by a series of ages, in which the use, first of stone, then
of bronze, and ultimately of iron for the manufacture of tools and
implements, indicate the development of industrial culture. The dates
which can be assigned to those periods vary with the locality; the
races in the more Northerly latitudes being later in their development.
In our own country, the Stone Ages may be said to date from 3000 B.C.
down to 1000 B.C., and the Early and Late Bronze Ages from 1000 B.C.
to 500 B.C., and from 500 B.C. to the commencement of the present era,
respectively.
It is not unlikely that in many places copper was largely used during
the Stone Ages and before the Bronze epoch, since it was only after
the art of making fire had been discovered that it became possible to
manufacture bronze, whilst native copper could be fashioned without
the aid of heat. Metallic relics of the Bronze Age, in the form of
arms, ornaments, and domestic implements have been found in widely
distributed localities.
The mention of copper occurs in the Hebrew Scriptures, the metal
being termed _Nehosheth_, from the root _Nahásh_, to glisten. This
was translated as χαλκὸς (_chalcos_) in the Septuagint, and _Aes_ in
the Vulgate; the Greeks and Romans using the terms, however, both for
copper and for the alloys brass and bronze.
According to Pliny, the Roman supply was derived chiefly from Cyprus,
and the metal thus came to be known as _Aes Cyprium_, which was
gradually shortened to _Cyprium_, a name afterwards corrupted to
_Cuprum_, from which are derived our modern terms _Copper_, the German
_Kupfer_, and the French _Cuivre_.
Copper was well known to the alchemists, and inasmuch as it was largely
obtained from Cyprus, an island dedicated to Venus, it was considered
to be the metal specially sacred to the Goddess, and was generally
known by that name in their writings, and symbolised by the sign
[symbol: circle with plus sign underneath]. The production of metallic
copper on iron by the action of certain liquors from the Hungarian
mines and other localities, was likewise known to the alchemists, and
was a constant source of inspiration to them; the changes were regarded
for some hundreds of years as examples of the transmutation of the
elements, until Boyle showed that it was necessary to introduce copper
into such solutions before that metal could be precipitated from them.
=The Development of the Copper Industry.=—The mining and smelting
of copper ores on a primitive scale have been carried on from time
immemorial; these operations were certainly practised in Greek and
Roman days, and the deposits of Britain are said to have been known to
the Phœnicians so far back as 1000 B.C. Percy refers to the finding
of lumps of copper weighing 42 lbs., carrying a Roman inscription;
this metal was found in close proximity to mines in North Wales, which
yielded an easily reducible ore, and he concluded that this was smelted
_in situ_ by the Romans.
There are undoubted records of copper mining in this country in the
time of Edward III., and in that of Elizabeth; whilst the first
authentic accounts of copper smelting date also from the latter
period, relating to South Wales. It appears that one of the earliest
establishments was situated at Neath—a fact recorded in a publication
of 1602. The works probably existed for a century before that date,
and the copper smelters at Swansea were established about 120 years
afterwards.
The processes employed for the primitive smelting of copper ores
were, to a large extent, of the same nature as the crude operations
practised generally for the extraction of metals in remote ages and
by primitive races, as recorded from time to time by travellers and
explorers. The furnace-hearth was a hole in the ground, working usually
on oxide ores with charcoal or wood as fuel. This primitive furnace was
later developed, by the addition of walls for enclosing the charge,
until the “shaft furnace” provided with an air blast of some kind
was attained. The sulphide ores presented rather more difficulty in
their treatment, but the production of metallic copper from sulphide
materials by super-oxidation, in a process akin to the bessemerising of
to-day, was developed in Japan centuries ago, and has been described by
Professor Gowland.
It would appear that during the middle ages, the art of reducing
copper ores to metal on a comparatively large scale was practised
simultaneously in Britain and in Central Europe; first by primitive
methods similar to those indicated above, developing later by
successive improvements into the employment of small blast furnaces.
By about 1700, however, the methods diverged, and it is interesting
to note that the different styles of working then introduced have
persisted, until recent years, as the methods typical of these two
parts of the world. In Wales, where the well-known furnace coal was one
of the characteristics of the locality, as it still remains to-day, the
smelting processes developed along the lines of reverberatory practice,
for which such fuel is eminently suited, and this resulted in the
establishing of the representative Welsh process. On the other hand,
the enormous forests of Central Europe furnished wood suitable for the
making of charcoal, a type of fuel which necessitates close proximity
with the furnace charge, so that in these localities smelting was
carried out in the shaft furnace, which gradually developed into the
small blast furnace. At the present time, the solid fuel suitable for
reverberatory practice is only obtainable in very small quantities in
Central Europe, and the characteristic method employed there for copper
smelting is that in which small blast furnaces are used, except that
charcoal has been largely replaced by coke as the fuel.
It is probable that the early ore furnaces of the primitive
blast-furnace type in Britain were worked by Germans experienced in
that class of work, just as at a later period in the history of the
industry, Swansea coppermen were to be found in all parts of the world
teaching other nations their art. Gowland reproduces a letter, dated
January, 1583, protesting against the introduction of this foreign
labour, whilst a second letter, dated July, 1585, which is also quoted,
is of particular interest, as it gives evidence of a remarkable
knowledge of the art of smelting, and, whilst illustrating an important
feature of modern practice, indicates also the manner in which an
astute smelterman was able to work profitably with difficult material
so long ago as three and a quarter centuries.
The letter is to the following effect:—
“ULRICKE FROSSE to ROBERT DENHAM. _4th July, 1585_.
“To his loving friend, Robert Denham.
“Friend Denham,—I have me heartily commended unto
you, you shall understand it we did lack ore more than
14 days ago, for we have found out a way to smelt 24
cwts. of ore every day with one furnace, the Lord be
thanked, and if we may have ore enough from your side
we may, with God’s help, melt with two furnaces in 40
weeks 560 tons of ore, having reasonable provision
made for it, desiring you from hence-forward to send
such ores as you have with as much speed as maybe, not
caring what ore it is. Your ore of St. Dines is very
hard to melt it, hoping we will overcome it what St.
Ust ores will do, we long to see it.
“This I rest, the Lord send you good success with
your mines. And so I commit you to God. From Neath, the
4th of July, 1585.
“Your friend,
“ULRICKE FROSSE.
“When you do send any more ore, if you can, send
of all sorts, the better it will melt and with more
profit.”
The sound principle of obtaining, when possible, one class of copper
ore for the purpose of fluxing off the gangue from ore of another
class, was thus recognised as a profitable feature of practice from
comparatively early times.
Copper mining and smelting in Staffordshire dates back a considerable
time, certainly prior to 1686; the mines were situated at Ecton, and
the smelter was at Elleston, near Ashbourne, where small blast furnaces
were employed. Copper smelting in Lancashire, which is nowadays
conducted on a comparatively extensive scale, appears to have commenced
in 1720 with Cornish ores and smaller importations from the West Indian
and American Colonies. During the 18th century, the chief supply of
the world’s copper ore came from the Cornish mines, which even at
that time, were deep and extensive. It seems, however, that for some
peculiar reason, the Cornishmen were unable to smelt these ores with
profit, nor indeed, to do more with them than to send the material to
South Wales to be treated. There are numerous explanations for their
failure, which have been discussed exhaustively by Percy.
The centre of the copper smelting industry thus came to be located
in the South Wales (Swansea) district, where circumstances were very
favourable. The study of local conditions is one of great importance
for metallurgists, and since this case affords a good example, it will
be of value to refer briefly to those circumstances which rendered the
Swansea district such an excellent centre for the industry.
The extensive collieries in the locality rendered available an abundant
supply of suitable fuel at a low price, and many of the smelters held a
financial interest in them. The large coal was profitably used for home
consumption or export, and the small, which, though dirty, still gave
the long flame required, was very suitable for smelting work, and was
reserved for that purpose.
Further, Swansea was an excellent seaport, situated at a short distance
only from Cornwall, the chief source of ore, and was also readily
accessible to vessels carrying cupriferous ores and products from
South America, Australia, and other parts of the world. This was a
great advantage, in that the Swansea copper smelters, having a large
variety of ores at their disposal, some with basic gangue, others with
siliceous gangue, were in a position to make up furnace charges which
were more or less self-fluxing, and thus avoided the necessity for
purchasing and using barren fluxes. The finished products were also in
a most convenient centre for distribution, at the seaport of Swansea.
At the end of the 18th century, Great Britain was producing 75 per
cent. of the world’s copper, the Cornish mines supplying most of the
copper ore, and the Swansea smelters extracting most of the world’s
supply of metal. Stevens has summarised the position for 1799, showing
that “from the Cornish ores 4,923 tons of refined copper were produced,
and from the Welsh ores of Anglesea 2,000 tons. The great Mansfeld
mine in Germany produced only 372 tons in that year, Spain’s output
was insignificant, and in the United States only a few tons were made.
Russia and Japan probably ranked next to Great Britain as producers,
small amounts of ore from Austria, Scandinavia, and Italy made up the
remainder. Thus at the commencement of the 19th century, the copper
resources of the United States, Spain, Chili, Mexico, Australia,
Tasmania, Canada, and South Africa, which now supply over 90 per cent.
of the world’s metal, were either undeveloped, or only yielded a few
tons each; Great Britain, which produced nearly 7,000 tons of copper at
that time, extracted from its own ore supplies, a hundred years later,
only 550 tons.”
It will be remembered that it was in connection with the development of
Cornish copper mining that the use of steam power in engineering was
introduced and successfully worked out. On account of the increasing
depth and extension of the Cornwall mines, the problem of disposing
of the underground water became urgent, and led to the introduction
of steam engines for driving the pumps, the Newcomen engine being
installed on the Wheal Fortune Mine in 1720. The success of this engine
led to increase both in depth and in extent of the workings, until it
became impossible to cope with the pumping requirements by this means.
At the right moment Watt brought out the modern steam engine, and the
first Watt engine was erected in 1777 at Chasewater, in Cornwall. It
was the introduction of these improved methods of pumping which have
made possible the successful development of present-day mining. Not
only has the steam engine thus led to an increase in the supply of
copper, by enabling the opening up of vaster deposits to be undertaken,
but the development of engineering science which it has brought about,
has caused a further consumption of the increasing quantity of copper
which it has helped to render available for use.
During the first half of the 19th century Great Britain retained its
position as the chief copper producer of the world, and the Swansea
smelters possessed advantages such as have been rarely enjoyed by any
other body of manufacturers. They were able to impose what conditions
they pleased on the producers and sellers of copper ore, as well as on
the consumers of the metal, and as business men, were not slow to avail
themselves of their opportunities to the greatest possible extent,
strengthening their position by the formation of a combination known as
the Associated Copper Smelters of Swansea, which controlled the price
of the metal from 1850 to 1860. Percy gives an interesting account of
the terms imposed by them under the name of returning charges, etc., as
well as of the conditions of sampling, analysis, and sale, which were
strongly in their favour.
During these years of monopoly, the smelters were, on the whole,
conservative in tendency from the metallurgical point of view, and
few great developments in either processes or methods were devised:
nevertheless, they enjoyed great prosperity, and their business
attained such dimensions that Swansea remains one of the greatest
centres of smelting industry in the world. The Welsh smeltermen had,
moreover, acquired such proficiency in furnace management, and such
knowledge of the working and control of copper charges, that their
reputation had spread to all quarters of the world.
Though from 1840 onward, the British copper mining industry commenced
to decline, still for 20 years longer the Swansea smelting works
prospered more and more as new mines were being opened abroad and thus
furnished a constantly increasing supply of rich copper ore, cheap to
purchase and easy to smelt.
It was this development of foreign copper resources, and the
unsatisfactory conditions which the producers received at the hands
of the smelters, which was the cause of the eventual displacement of
Swansea from its position as the leading seat of copper manufacture.
In 1830, the production of copper ore in Chili had commenced and
developed rapidly, Chili soon becoming one of the chief suppliers of
ore to the Welsh smelters, whose independent attitude led to the first
introduction of the copper-smelting industry on any large scale in
America. Owing to the sailing conditions of the time, the simultaneous
coming into port of several ships laden with ore, instead of their
arrival at regular intervals, enabled purchases to be made by the
smelters at a remarkably low figure, the standard price of the metal
being subsequently raised. Mine-owners commenced to seek for a remedy,
their ultimate endeavour being to substitute, for the exportation of
their ores, smelting operations at or near the mines themselves. In
1842 Lambert introduced reverberatory furnaces into Chili, and so great
was his success, that in a short time they were in use throughout
that country. In 1857 he erected the first blast furnace in Chili,
and the smelting industry thereupon grew so rapidly that, whilst from
1856 to 1865 the copper exports from Chili were in the proportions of
ore 21 per cent., regulus 38 per cent., and bars 40 per cent., they
subsequently became ore 1½ per cent., regulus 3½ per cent., and bars
95 per cent. The ultimate effect was a widening of the market for the
finished Chilian product, so that Continental purchasers were enabled
to obtain their supplies of metal direct, instead of being obliged
to purchase from the Welsh smelters on the unsatisfactory terms then
prevalent.
In 1842 the first large copper mines of Australia (Kapunda and later
Burra Burra) were discovered, but developed slowly; and in 1844 the
first copper mines of the Lake Superior district began work—on oxide
ore, not on native metal.
In 1850 an enormous development in the Chilian mines commenced, half
the world’s copper being produced from this source; in 1859–60 the
Spanish mines at St. Domingo (Mason and Barry) were re-opened, as
well as the Portuguese mine, the Tharsis. These mines were in reality
operated in order to supply the wants of the sulphuric acid industry,
the ore residues being subsequently smelted for copper at Swansea. In
1862, however, the Henderson wet process for copper was introduced,
for which these materials were very suitable, and the Spanish and
Portuguese supplies became of considerable importance, soon afterwards
coming under the control of a Scottish company.
The competition from these new and abundant supplies of rich ores from
Chili, Spain, and Portugal severely injured the production from the
British mines; increasing supplies led to a fall in the price, and one
native mine after another shut down, the British supply diminishing
with considerable rapidity.
In 1866 the great Calumet and Hecla mine at Lake Superior commenced
operations, and speedily became one of the most important sources of
copper in the world; the Moonta and Wallaroo mines in Australia opened
about the same time, and in 1873 the Arizona mines started producing.
In 1876 the enormous Spanish mines at Rio Tinto were re-opened, and
soon rendered available large quantities of ore. Later, the Tasmanian
supplies entered the markets.
In 1880 a remarkable development in copper mining occurred with the
discovery of the Butte camp in Montana; this is now the greatest
producer in the world.
The later extensions of the copper mining industry occurred in Utah,
Tennessee, and Queensland, whilst within recent years the most
important work on a large scale has been commenced in Tanganyika, in
Nevada, and in Siberia.
The developments in the smelting industry in most of these localities
have proceeded, until the last few years, on very similar lines. During
the first periods following the opening up of mines and works, ore
was shipped to the custom smelters, most often to Swansea; where, in
the early days, many of those connected with the smelting works had
some sort of financial interest in the foreign mines. Later, the ore
underwent its first smelting to matte in the mining district itself,
the matte product being then shipped East for treatment, thus saving
much of the freight-charge on useless gangue, as well as smelters’
heavy returning charges, etc. At a later period the smelting operation
was carried to a still further stage in the mining district, crude
blister copper only being sent to Swansea or elsewhere to be refined.
Gradually, electrolytic refineries were established somewhat nearer to
the mining districts, and in the natural course of events, and where
local conditions are not prohibitive, the probability is that the whole
cycle of operations from mining to the production of refined market
metal will be carried out at the great camps themselves.
At present, however, this is not generally the case, since the
conditions under which the enormous refineries in the Eastern States
of New York, New Jersey, and in Baltimore, etc., operate, allow of
the cheaper production of electrolytic copper at points nearer to
the distributing markets. At Anaconda, indeed, the fully-equipped
electrolytic plant was shut down, owing to the commercial conditions
such as have just been indicated, having rendered the refining of
the anode copper at the Eastern refineries more profitable than
electrolytic treatment on the spot.
=The Chief Features in the Development of Modern Copper Smelting
Practice.=—In the early days of copper smelting, the reduction of the
oxidised ores, which were then chiefly available, was not a problem
of very great difficulty, although losses in slag were likely to be
very high, and the operation generally wasteful. When, however, mines
became deeper and sulphide ores had to be smelted, the problem became
rather more complicated. In the first stages of development, such
ores were probably roasted until as much sulphur as possible had been
driven off, leaving practically an oxide charge to be treated by the
older reduction methods involving the attendant extravagance in fuel
consumption and large losses of copper in the slag.
From these crude and wasteful methods the Welsh process was gradually
worked out, and it will ever rank as one of the finest examples of
highly developed smelting practice in the history of metallurgy,
particularly when the times and working conditions are borne in mind.
The process having received such full treatment from most of the common
text-books, it is not proposed to review it in detail here, since,
moreover, it has been largely superseded by more modern processes.
As will be explained later, copper smelting of sulphide ores is
essentially a fractional oxidation—chiefly of iron and sulphur—followed
by the slagging or elimination of extraneous constituents of the ore.
The Welsh process embodied a series of roastings and slaggings which,
though most admirably adjusted for a substantial concentration of the
copper in each succeeding product, allowed of the formation of slags
in the first stages which carried but comparatively little copper, on
account of the low tenor of the matte; whilst the slags in the later
stages of the process, containing more copper on account of their
association with higher grade matte, were made in such relatively small
quantity that their re-treatment for the recovery of these values did
not involve very much loss of efficiency in the furnace operations.
Later modifications of the process were chiefly devised with the view
to reducing the number of operations, by eliminating the successive
roasting stages, for which purpose oxidised materials, such as roasted
or oxidised ores, were added to the charge.
The Best-Selecting process, and the Nicholl and James process are
likewise valuable and ingenious modifications of the Swansea method for
special work.
In general, however, up to 1880, there had taken place but little
change in principle from the older methods of smelting. The chief
improvements involved a slow change in furnace size, and progress in
several details in practice. The more important of these advances were—
(_a_) _In Roasting Practice._—=1865.= Introduction
of the mechanically driven furnace (the Brückner cylinder);
not, however, adopted for copper smelting till many years
afterwards. Later—Arrangements for using roaster gases for
sulphuric acid manufacture.
(_b_) _In Reverberatory Furnace Smelting._—=1861.=
Gas firing introduced, but with very little success for
copper smelting, even at the present day.
(_c_) _In Blast-Furnace Smelting._—Several very important
changes were introduced in the construction of furnaces.
=1863.= Elongation of the furnace.
Rachette in Germany introduced the elliptical blast furnace. (Intended
first for lead smelting; rapidly adopted for copper matte smelting.)
=1875.= The water-jacketing of blast furnaces.
The Piltz water-jacketed furnace was likewise first employed in lead
smelting, and subsequently introduced into copper smelting practice.
The principle had, indeed, been utilised in certain branches of iron
smelting before this date, but for non-ferrous work the idea was new.
Although the method of water-jacketing was recognised as leading to
great improvement in the working of the furnace, its use was at first
somewhat restricted, owing to various practical difficulties, and the
ultimate great success was effected when in American practice, the plan
of working the two principles of elongated furnaces and water-jacketing
in conjunction, was adopted.
Commencing from 1880, and onwards, however, when production in the Far
West began, enormous advances have been made, both in connection with
the principles of working as well as in practical operation. These
include—
(1) Enormous increase in the size and capacity of furnaces
of both the reverberatory and the blast-furnace type.
(2) The application of the Bessemer process to copper mattes.
(3) The development of the pyritic smelting principle.
(4) The adoption of electrolytic refining.
(5) The use of mechanically rabbled roaster furnaces.
(6) The manufacture of sulphuric acid from blast-furnace gases.
(7) The blast-roasting and sintering of sulphide fines.
With an increased output of ore from the mines, and with increased
consumption, stimulated by the growth of the electrical industry, the
demand for metal increased so quickly that developments naturally
followed with a view to an augmented and rapid production by more
efficient and scientific processes; especially since increased
competition and poorer ore supplies necessitated a very decided
lowering of the costs of production. To meet the enormous present-day
demand for metal with the older methods and furnaces would have been
impossible. The greatest stimulus to the adoption of these new or
modified processes was the shifting of the chief producing centres
from the older and more conservative influences to districts like
the then newly awakening West, where, with ever-increasing—almost
limitless—supplies of ore available, and free from the necessity of
considering the capital invested in old plants, the men in charge of
the work, untrammelled by old smelting customs which might stand in the
way of rapid progress, were in a position to develop their ideas with
originality and vigour.
There may, nevertheless, be recalled the important share which British,
and especially Swansea, workmen had in this great development of the
industry. At many of the greater smelters in these new districts, Welsh
furnacemen are still to be found, and large numbers went abroad in
former days to take charge of such work, especially during the critical
early stages. The principles underlying these modern improvements were,
in many cases, first worked out by scientists in Europe.
=The Price and Cost of Production of Copper.=—The price of copper
has been influenced to an enormous extent by financial speculation,
so that until recent times it has fluctuated very considerably from
year to year, the curve in fig. 1 relating to Best Select copper,
indicating this variation over a considerable period. The price of the
other qualities of commercial copper follows this line fairly closely,
electrolytic copper being from £2 to £4 per ton lower, and standard
copper £3 to £6 per ton. The average value of the standard refined
metal at the present time (December, 1911) is about £56 per ton in
London, and about 12 cents per pound in New York.
On three occasions during the past century, and once at least during
the past decade, the market price of copper has been directly affected
by more or less artificial conditions consequent on financial
manipulation. The first of these instances was the 1850–1860 period,
when the Welsh smelters held the monopoly of the copper trade, and
were in a position to fix their own price; the second was during the
French combination of Secretan during 1887–9, which, as a result of
mere market speculation, caused fluctuations of price which amounted on
one occasion to no less than £35 per ton within twenty-four hours. The
third instance was created by the American combine.
[Illustration: Fig. 1.—Fluctuations in the Price of Best Select
Copper.]
In 1899 the Amalgamated Copper Company was formed in the United States.
This corporation was established in view of the enormously increasing
production of the West, and of the extensive development of electrical
industry which involved a greatly increased consumption of copper; and
it was probably designed to control the world’s copper industry. Prices
were raised gradually for some time, but in 1901 the Trust, as then
constituted, failed, owing largely to trade depression in Europe. Heavy
losses resulted, as well as expensive law suits, and the price of the
metal dropped again with great rapidity. Trade subsequently revived
and expanded, the consumption of copper increased and appeared to
overtake the rate of production, whilst stocks diminished and the price
advanced, until, in 1907, copper was sold at well over £100 per ton.
The American financial panic in the autumn of that year again reduced
prices to a comparatively low figure, and they have, on the whole,
remained fairly steady since, though showing a tendency to decrease.
Production has, meanwhile, increased very largely, and a steady price
of 12 to 13½ cents per pound yields handsome profits to most of the
larger concerns. The present situation in the copper market is such
that the enhanced production has again resulted in an accumulation of
stocks, which has occasioned restricted output on the part of many of
the principal smelters until briskness of trade development shall call
forth increased consumption and more satisfactory prices.
The question of price is one involving certain considerations to which
attention may be drawn. The present conditions and the comparative
steadiness in the copper market have been shown in a recent review to
result in part from:—
(1) The concentration of the copper industry in a few
strong hands, which, whilst maintaining healthy competition,
keeps the market free from such outside pressure as would
reduce the price too much, and by restricting unprofitable
output, brings production and consumption into equilibrium,
making for stability.
(2) The comparative cheapness of money, which has allowed
of the financing for large production, with the prospect of
absorption not being long delayed.
At the same time, some of the richer and more cheaply worked mines of
former times are gradually approaching exhaustion—recent instances of
this will be readily recalled, whilst the disadvantages of having to
work lower-grade deposits at greater depth have also tended to increase
the price of metal. These conditions, on the other hand, have been
counterbalanced by improvements in the mining and metallurgical
processes concerned, by the opening up of new districts, and by the
economies resulting from amalgamation of interests, involving closer
organisation and enormous outputs of material.
Apart from finance, two of the factors most likely to affect the price
of the metal considerably are the possible replacement of copper for
electrical transmission purposes by conductors of other metals; and
further, the enormous prospective production in the newer districts,
such as Utah, Nevada, and Tanganyika, in the course of a few years.
The cost of production of the metal is so dependent on local and
general circumstances as not to admit of analysis in this place.
Questions of locality, transport facilities, proximity to supplies
of every kind, problems of labour, capitalisation, bye-products, and
numerous similar considerations have such an important bearing on each
individual case as to convey a definite meaning only to the man on
the spot. In the same way, detail costs of each stage of the copper
smelting processes are influenced by similar circumstances.
Broadly speaking, the average total cost of production and marketing
at present may be taken as being somewhere about 10 cents per pound
of copper; in certain specially favoured cases, 9, 8, or even 7 cents
per pound. The newly opened low-grade “porphyry” camps at Utah and
elsewhere, which have been commenced under an enormous capitalisation,
anticipate a production at a cost of about 6 cents per pound when
steady and normal running is in progress.
A recent analysis gives interesting information with regard to the cost
of production estimated at different plants. Of the American output of
about 480,000 tons in 1909—
Almost 3·5 per cent.
was produced
at a cost of 7·14 cents per lb. (Nevada).
1·8 " 7·98 " (Baltic, Superior).
10·5 " 8–9 " (Utah, etc.).
48·3 " 9–10 " (Boston and Montana,
Calumet and Hecla, etc.).
9·0 " 10–11 " (Utah Consolidated,
Tennessee, etc.).
20·0 " 11–12 " (Anaconda, Arizona, Cananea).
1·8 " 12–13 "
1·1 " 13–14 "
1·4 " 14–15 " (Tamarack).
1·1 " 15–16 "
1·1 " 16–17 "
0·1 " 17·09 "
=Copper Statistics.=—The outstanding features which attract
attention in the statistics of copper production will be most readily
seen from the curves of fig. 2. The enormous increase within recent
years in the total output of metal, and the overwhelming proportion
produced by the United States of America, is clearly indicated. The
curves also show the practical extinction of the native supply of Great
Britain and the steady output of Spain and Germany.
An analysis of the total production for the year 1910 is given in the
following Table I.:—
TABLE I.—THE PRODUCTION OF COPPER (Short Tons of 2,000 lbs.).
1909. 1910.
─┐
U. S. A., 549,114 543,125 │
Canada, 26,998 28,801 │ 1909. 1910.
Newfoundland, 1,546 1,210 ├─ North America,
Mexico, 63,085 68,899 │ 644,058 645,927
Cuba, 3,315 3,892 │
─┘
─┐
Argentina, 672 336 │
Bolivia, 2,240 2,800 ├─ South America,
Chili, 40,079 39,463 │ 60,911 63,101
Peru, 17,920 20,502 │
─┘
─┐
Spain and Portugal, 58,447 56,386 │
Germany, 25,150 27,675 │
Russia, 19,880 24,987 │
Norway, 10,170 11,676 │
Hungary, 5,152 5,550 ├─ Europe, 127,283 135,738
Sweden, 2,240 2,240 │
Italy, 3,052 3,606 │
Austria, 1,809 2,386 │
Turkey, 896 672 │
Great Britain, 487 560 │
─┘
Japan, 52,640 51,520
Africa, 16,738 17,030
Australasia, 38,528 45,153
_______ _______
Total, 940,158 958,469
═══════ ═══════
[Illustration: Fig. 2.—Annual Production of Copper.]
In Table II. is indicated the distribution of the American production
among the various States.
TABLE II.—NORTH AMERICAN PRODUCTION OF COPPER
(in Short Tons of 2,000 lbs.).
1909. 1910.
Alaska, 2,028 2,504
Arizona, 146,021 149,803
California, 26,679 22,897
Colorado, 5,244 5,063
Idaho, 3,885 3,108
Michigan, 113,624 110,700
Montana, 156,918 143,121
Nevada, 25,917 31,944 (about 6,000 tons in 1908)
New Mexico, 2,567 1,816
Utah, 50,219 62,521 (about 35,000 tons in 1908)
Wyoming, 44 90
South and East, 11,409 9,098
Other States, 1,973 463
———- —-———-
Totals, 546,538 543,125
There will be noticed a decline in the production of the United States
during the year 1910, resulting from the present movement to restrict
output whilst the large accumulated stocks of metal are being absorbed.
The movement is probably more or less temporary, and is being largely
directed by American financiers who are endeavouring to bring about an
international agreement on the subject.
Regarding the American output, the marked movement for curtailment in
Montana has reduced the output of that State to such an extent, that
the position it gained in 1909, of being the greatest producing State
once more reverts to Arizona. The increases from Nevada and Utah, in
which developments on a large scale are commencing, may be noted.
References.
Percy, John, “Metallurgy (Copper).”
Gowland, William, Presidential Address,
_Trans. Inst. Mining and Metallurgy_,
vol. xvi., 1906–7, pp. 265–291.
Stevens, H. J., “The Copper Handbook.”
Brown, N., and Turnbull, C. C., “A Century of Copper.”
_Engineering and Mining Journal_, “Copper Production.”
May 6th, 1910, p. 891.
_Mineral Statistics of the United Kingdom._
_Mineral Industry._
LECTURE II.
The Uses of Copper: as Metal and as Alloy — The
Physical Properties of Copper — Effects of
Impurities — Mechanical Properties — Chemical
Properties.
=The Uses of Copper.=—Generally speaking, the industrial
applications of copper involve its employment in two forms:—
(1) As metal.
(2) As a constituent of alloys.
The more limited use in the form of copper salts is of chemical rather
than of metallurgical interest.
Copper in the metallic form is employed for three classes of work:—
(_a_) For electrical purposes.
(_b_) For engineering purposes.
(_c_) General industrial uses.
(_a_) _Electrical Uses._—Of late years the marked growth in the
consumption of copper has arisen very largely from its usefulness as
a conductor of electricity; the increased demand for the metal with
the development of electrical enterprise being a well-marked feature
in industrial progress. It is estimated that from 60 to 70 per cent.
of all the copper produced is utilised for this purpose, and metal is
specially prepared and sold under the designation of “high-conductivity
copper.” The demand has, to a large extent, increased irrespective of
price up to recent years, owing to the necessity of employing copper
for such purposes, though the natural economic factor that an enhanced
price of the metal tends to some discouragement of expansion and
of fresh electrical enterprise, has exerted considerable effect in
checking consumption.
It is merely necessary to enumerate some few of the present aspects
of electrical industry in order to realise the enormous absorption
of copper in this connection, as, for instance, electrical traction,
lighting, and power, the telegraph, and the telephone. With reference
to the use of the metal for this work, it is important that certain
mechanical as well as electrical requirements should be fulfilled,
for in many branches, considerable strength of the material is
also requisite. The demand of the electrical engineer is that as
a conductor, the copper shall offer a minimum of resistance to the
passage of the current, and for this requirement the metal must be
in a condition of very great purity. With but few exceptions, this
necessitates the purification of the copper by electro-deposition.
Electro-deposited metal as produced at the refineries is, however, not
immediately suitable for drawing into wire, owing to the weakness and
porosity inherent in the material prepared by this method. It must,
therefore, be melted, brought to pitch, cast into bars, and these bars
transformed into wire, which operations require to be conducted with
much care in order to keep the metal in as pure a condition as possible
for its work. It may be noted that within recent years, several
processes, notably those of Cowper-Coles and Elmore, have been put
into operation for the direct manufacture for electrical purposes, of
electrolytic-copper wire of the requisite strength.
The mechanical qualities demanded of the metal for such purposes as
telegraph work may be indicated by the two specifications of wire for
the British Post Office, which are appended:—
A. _Post Office Specification._
=Weight=, 150 lbs. per mile.
=Minimum diameter=, ·95½".
=Maximum diameter=, ·98".[1]
=Minimum breaking strain=, 490 lbs.
=Minimum number of twists=, 25 in 3 inches.
=Wraps required=, 6 times round wire of its
own diameter, unwrapped, and again wrapped without breaking.
=Maximum resistance per mile at= 60° =F.=, 5·857 ω.
B. _Post Office Specification._
=Weight=, 500 lbs. per mile.
=Minimum diameter=, ·135¼".
=Maximum diameter=, ·138¾".
=Minimum breaking strain=, 950 lbs.
=Minimum number of twists=, 30 in 6 inches.
=Wraps required=, 6 times round wire of its
own diameter, unwrapped, and again wrapped without breaking.
=Maximum resistance per mile at= 60° =F.=, 2·928 ω.
The following figures afford some indication of the increasing demand
for copper in two branches only of electrical industry:—
1902. 1907.
Mileage of wire for telegraph purposes, 3·9 5·3
" " telephone purposes, 10·9 28·2
(in million of miles)
(_b_) _Engineering Uses._—Metallic copper finds application in marine
shipbuilding and engine work, as well as in railway and locomotive
work, where the metal is particularly employed for steam pipes, and
for fire-box plates and stays, sometimes also for boiler tubes, on
account of its high conductivity for heat, combined with toughness.
The questions of suitable composition, and the other requirements
of the metal intended for these purposes, has been a subject for
discussion by some of the leading marine and locomotive engineers.
Useful information on the subject will be found in the reports of some
of these discussions at the Institution of Mechanical Engineers.
The following tests are required for copper plate (best quality)
intended for locomotive fire-boxes on the Lancashire and Yorkshire
Railway, taken from standard specifications given by their Chief
Mechanical Engineer at the Institute of Metals:—
_Bending Test._—Pieces of the plate shall be tested both
cold and at a red heat by being doubled over on themselves—
that is, bent through an angle of 180°—without showing
either crack or flaw on the outside of the bend.
_Flanging._—Plates must not show any defects in flanging.
_Tensile Test._—Ultimate breaking load, 14 tons per square
inch; Elongation, 35 per cent. in 8 inches.
_Analytical Test._—To be made at contractor’s expense.
The copper upon analysis to give the following results:—Arsenic, not
less than 0·35 per cent. nor more than 0·55 per cent.; other foreign
elements, exclusive of combined oxygen, not to exceed 0·25 per cent.
Clauses are also inserted as to stamping, inspection, and the giving of
testing facilities.
Typical analysis of such plates show—
Copper, 99·30 per cent.
Arsenic, 0·43 to 0·51 per cent.
Oxygen, 0·1 per cent.
Impurities, chiefly antimony, lead, iron, nickel, tin, and sulphur, not
exceeding 0·25 per cent.
The average test on a number of plates gave—
Tensile strength, 14·66 tons per square inch.
Elongation on 8 inches, 43·36 per cent. of original length.
Contraction of area, 45·9 per cent.
Close bend test, Double.
The effect of temperature and the influence of impurities on the
mechanical properties of the metal intended for engineering purposes
are of very great importance, and much attention has been devoted to
researches in this subject, particularly by Milton and Le Chatelier,
whose published experience gives important information of much
practical value. The main conclusions arrived at from practice have
had reference to the general effects of impurities in hardening the
metal, and the general tendency of heat to soften it and to increase
the ductility. The diverse effects of different impurities on strength
and ductility will be reviewed in detail at a later stage.
(_c_) _General Industrial Uses._—Copper as metal is also employed to
a considerable extent in certain important industries, as in textile
manufacture, where it is used for the rollers in calico-printing; and
it is in general industrial use in the form of copper heaters, vats,
coils, pans, and the like, and occasionally also for roofing and
sheathing.
=Uses of Copper Alloys.=—Between 20 and 30 per cent. of the copper
produced is employed in the form of alloys. The more important of these
are:—
=Brasses=; alloys of copper and zinc.
=Bronzes=; chiefly alloys of copper and tin.
=Coinage Alloys=; of gold and silver with copper.
=German Silver=; alloys of copper, nickel, and zinc.
=Special Bronzes=; alloys of copper with such metals
as aluminium and manganese.
It is further not unlikely that several classes of ternary alloys,
at present still under investigation, may have important industrial
application in the future. Among such alloys may be mentioned the
copper-aluminium series alloyed with other metals, Monel metal and the
Monel steel series, etc.
Of the above alloys, the brasses are by far the most widely used. It
may be recalled that the advantages possessed by alloys of copper and
zinc are in large measure due to their increased strength and hardness;
to the fact that they are more fusible, and more fluid when melted, and
so give good castings; that they are characterised by a good colour and
high lustre, as well as by the factor of cheapness resulting from the
addition of a less costly metal—zinc—in their manufacture.
The uses of the copper alloys may also be arranged in two classes—(_a_)
engineering uses, and (_b_) general uses. Of the brasses, those
containing upwards of 70 per cent. of copper may be rolled cold, whilst
the alloys with less than 70 per cent. are hot-rolled.
In the engineering industry large quantities of 70/30 brass are
utilised in the form of condenser tubes, whilst for the multifarious
requirements of general engineering work, very considerable amounts
of brass of lower tenor are employed in the forms of taps, pipes,
fittings, etc.
Muntz metal, the 60/40 brass, finds extended application for the
sheathing of ships, whilst the employment of brass and of the other
alloys for all manner of articles of general utility is a matter of
common knowledge.
The close connection between properties, constitution, and the
equilibrium diagram of these various classes of alloys has become
manifest to a marked degree within recent years, and the effects
of thermal treatment partly in modifying their constitution, and
thereby the properties, and also in controlling the condition and
distribution of the constituents, are at the present time having an
important bearing on the manipulation of these alloys in the industries
manufacturing them and adapting them for their various uses. The study
and application of these equilibrium diagrams are highly important to
those who have to deal with these alloys on an industrial scale.
[Illustration: Fig. 3.—Equilibrium Diagram, Cu-Zn Series.]
=The Properties of Copper.=—The properties of the metal which render
it of such service in the arts and industries are mainly its high
electrical conductivity, its great ductility, malleability, and
toughness, which enable it to be readily worked up into the different
forms in which it is employed, its high thermal conductivity, and its
resistance to the various agencies which lead to corrosion. These
are consequently the properties to which close study is directed.
Of perhaps still greater importance is a knowledge of the influence
exerted upon these properties by the circumstances which usually attend
working practice; such as, for example, the various common impurities,
and the variations of temperature, as well as the previous mechanical
and thermal treatment. These can only be indicated in general terms
here, references to authorities on the different branches being given
later.
TABLE III.—INFLUENCE OF IMPURITIES ON THE ELECTRICAL CONDUCTIVITY.
┌─────────────┬───────────────────────┬───────────────────────┐
│ │ Addicks. │ Johnson. │
│ ├─────────┬─────────────┼─────────┬─────────────┤
│ │Impurity.│Conductivity.│Impurity.│Conductivity.│
│ │Per cent.│ │Per cent.│ │
├─────────────┼─────────┼─────────────┼─────────┼─────────────┤
│Pure copper, │ .. │ 101 │ .. │ 101 │
│Copper with— │ │ │ │ │
│Aluminium, │ 0·006 │ 98·6 │ 0·01 │ 99·7 │
│ │ 0·109 │ 66·8 │ 0·02 │ 98·8 │
│ │ 0·739 │ 43·5 │ .. │ .. │
│Antimony, │ 0·007 │ 99·6 │ .. │ .. │
│ │ 0·022 │ 97·2 │ .. │ .. │
│ │ 0·047 │ 95·4 │ 0·05 │ 96·9 │
│Arsenic, │ 0·004 │ 99·6 │ .. │ .. │
│ │ 0·007 │ 96·8 │ .. │ .. │
│ │ 0·013 │ 93·2 │ 0·04 │ 92·4 │
│ │ 0·140 │ 62·3 │ 0·06 │ 82·0 │
│Bismuth, │ 0·028 │ 99·6 │ 0·01 │ 95·7 │
│ │ 0·045 │ 99·3 │ .. │ .. │
│Cadmium, │ 0·062 │ 99·5 │ .. │ .. │
│ │ 0·113 │ 99·1 │ .. │ .. │
│ │ 0·427 │ 96·1 │ .. │ .. │
│Cobalt, │ .. │ .. │ 0·05 │ 92·0 │
│Gold, │ 0·089 │ 98·9 │ 0·05 │ 99·7 │
│ │ 0·149 │ 98·4 │ .. │ .. │
│ │ 0·317 │ 96·4 │ .. │ .. │
│Iron, │ 0·042 │ 96·8 │ .. │ .. │
│ │ 0·046 │ 92·9 │ .. │ .. │
│ │ 0·068 │ 89·6 │ 0·09 │ 98·8 │
│Lead, │ 0·083 │ 99·1 │ .. │ .. │
│ │ 0·052 │ 98·7 │ 0·06 │ 100·6 │
│ │ 0·347 │ 98·3 │ .. │ .. │
│Manganese, │ .. │ .. │ 0·02 │ 98·8 │
│Nickel, │ .. │ .. │ 0·05 │ 91·4 │
│Oxygen, │ 0·020 │ 100·7 │ .. │ .. │
│ │ 0·050 │ 101·4 │ .. │ .. │
│ │ 0·100 │ 100·5 │ 0·10 │ 99·8 │
│Phosphorus, │ 0·08 │ 52·3 │ 0·004 │ 98·5 │
│Platinum, │ .. │ .. │ 0·02 │ 93·6 │
│Silicon, │ 0·007 │ 99·4 │ 0·004 │ 99·7 │
│ │ 0·042 │ 99·0 │ 0·01 │ 98·4 │
│Silver, │ 0·003 │ 100·5 │ .. │ .. │
│ │ 0·137 │ 100·0 │ 0·05 │ 99·8 │
│ │ 0·340 │ 98·3 │ .. │ .. │
│Sulphur, │ 0·053 │ 100·0 │ 0·01 │ 98·5 │
│ │ 0·135 │ 99·0 │ .. │ .. │
│ │ 0·236 │ 98·9 │ .. │ .. │
│Tellurium, │ 0·065 │ 100·4 │ .. │ .. │
│ │ 0·181 │ 100·2 │ .. │ .. │
│ │ 0·405 │ 98·7 │ .. │ .. │
│Tin, │ 0·052 │ 97·6 │ 0·05 │ 100·5 │
│ │ 0·097 │ 92·7 │ .. │ .. │
│ │ 0·295 │ 79·8 │ .. │ .. │
│Zinc, │ 0·048 │ 98·3 │ 0·02 │ 98·5 │
│ │ 0·095 │ 96·3 │ .. │ .. │
└─────────────┴─────────┴─────────────┴─────────┴─────────────┘
PHYSICAL PROPERTIES.—The _colour_ of copper is familiar, being a fine
salmon pink. The _appearance of the fractured surface_ is a useful
guide in several respects as to the condition of the metal, and in the
process of manufacture the refiner relies upon this appearance as an
important criterion of the progress of the refining operation. Copper
containing an excess of oxygen, for example, has a purplish-red colour
and a coarse brick-like fracture; this is known as “_dry copper_,”
and the metal is brittle and commercially useless when in that form.
The ingot of dry copper is also characterised by a depression running
along the surface. _Tough copper_ (“tough-pitch”) the mechanically
useful variety resulting from the furnace-refining operation, possesses
a bright salmon-coloured fracture, finely granular to silky in
appearance, whilst “_overpoled copper_,” also brittle and industrially
valueless whilst in that condition, has a very light salmon-coloured
fracture, and is more coarsely fibrous.
The _melting point_ of copper is 1,083° C., and is slightly lowered by
the small quantities of impurity usually present in commercial metal.
Molten copper is of a pale apple-green colour. The _boiling point_
under ordinary conditions is about 2,300° C. (1,700° C. _in vacuo_).
The _electrical conductivity_ is of much importance. Copper ranks
second only to silver as a conductor, the relative conductivity of the
best copper being about 98 compared with silver as 100. The resistance
of 12 inches of pure copper wire, 0·001 inch in diameter, is 9·612
ohms. The conductivity of the metal is decreased by mechanical working,
and it follows the general straight-line law connecting conductivity
and temperature.
The effect of even small quantities of impurity on this property is
very marked, so much so that only the purest varieties are suitable for
electrical work, and for this reason electrolytic refining is often
a necessary operation in the manufacture of copper intended for this
purpose.
Table III. on preceding page, summarises the results of the work of
Addicks and Johnson, and indicates the effects of small amounts of
different impurities on the conductivity of the metal.
The notoriously destructive effect of arsenic on the conductivity is
very apparent.
The influence of most of the common impurities is of a similar nature,
and detailed investigations indicate that the effect is more or less
progressive as the quantity increases—within the limits usually present
in commercial metal. The results of Hiorns and Lamb’s experiments with
reference to arsenic and antimony are indicated in Fig. 4.
The _specific gravity_ of copper naturally varies according to its
condition and composition. When pure and in the worked state, its
density is 8·95; cast metal, more open and inclined to porosity, has a
density of about 8·2 to 8·6, depending on the purity, rate of cooling,
etc. Impurities lower the specific gravity.
The _conductivity for heat_ of the metal is high, being 898 compared
with gold as 1,000, and as a conductor it is two and a-half times more
efficient than iron. It is this property, combined with its toughness
and resistance to corrosion, etc., which largely determines its
employment for heaters, steam-coils, and the like.
[Illustration: Fig. 4.—Influence of Arsenic and Antimony on the
Electrical Conductivity of Copper.]
_Power of Dissolving Gases._—When molten, especially under reducing
conditions, the metal possesses the property, common to many others,
of absorbing gases such as carbon monoxide, hydrogen, hydrocarbons,
sulphur dioxide, etc., which are moreover, to a large extent insoluble
in the solid material, and are, therefore, often liberated at or about
the moment of solidification; though some may remain dissolved. This
action is one of the causes of the difficulty which is experienced
in making sound castings of the metal, particularly since the gases
mentioned are present in quantity during the poling and refining
operations. The presence of certain materials in the copper, as in
the case of steel, appears to reduce the dissolving power of the
liquid metal for these gases, or possibly to increase their solubility
when the copper is solidifying, and in this way tends to minimise
their injurious effects. It would seem that one of the functions of
the cuprous oxide, which is purposely introduced into the metal when
“bringing it up to pitch,” is to exert this action. The ridge in the
ingot of overpoled copper is, to some extent, accounted for as being
due to the effects of the evolved gases, and this appearance indicates
the absence of the requisite quantity of cuprous oxide necessary to
counteract the effect.
Copper is also supposed to be capable of holding certain quantities
of gas in solution after it has become solid, and the resulting
metal is more brittle and often commercially useless. Several of the
characteristics of overpoled copper probably arise from this cause also.
=Impurities[2] in Copper.=—In view of the marked influence of
impurities on the properties of metallic copper, it may be advisable in
this place briefly to review the results of recent scientific work as
to the condition in which they exist in the metal, thus offering some
clearer indication of the manner in which they affect the mechanical
and other properties. The common impurities in ordinary commercial
metal may be oxygen, arsenic, antimony, bismuth, lead, and to smaller
extents, iron, sulphur, tellurium, and selenium.
A factor of much importance is that the effect of two or more of the
common constituents when present together, may be of even greater
moment than that of each one separately, and in this connection
Hampe’s classical work should be consulted. The investigation of the
joint effects of impurities becomes so complex that systematic study
progresses but slowly. Metallographic work is, however, revealing
much evidence, and the researches in progress at present at several
laboratories will, when published, afford greatly increased knowledge
on the subject. Recent papers by F. Johnson give valuable detailed
information (see References, p. 34). The importance of oxygen in this
connection is particularly marked: its effects are profound, since in
addition to its own specific influence as oxide, it also brings about
chemical changes in some of the other constituents, thus leading to
the formation of entirely new compounds possessing quite different
properties. The beneficial influence of certain definite proportions
of oxygen in addition to the other constituents of commercial copper
is well known in practice, and has been systematically studied by
Hampe, and later by several other workers with more delicate means of
investigation at their disposal.
_Oxygen in Copper._—Molten copper has the power of dissolving its
oxide, Cu_{2}O. When the melted metal is exposed to oxygen, this oxide
is produced and passes into solution in the liquid, yielding a series
of binary alloys, of which the oxide acts as the second constituent.
The equilibrium diagram of the series, as worked out by Heyn[3] (see
Fig. 5), affords a good indication of these relationships, and throws
light on several features connected with the presence of oxygen in
copper.
[Illustration: Fig. 5.—Relations of Copper and Oxygen.]
It will be observed that when molten oxygenated metal containing less
than about 0·38 per cent. of oxygen solidifies, copper crystallises out
first, whilst later, in between the copper crystals, there solidifies
a eutectic of copper and cuprous oxide. This eutectic contains about
3·45 per cent. of cuprous oxide, equivalent to 0·38 per cent. of
oxygen; it melts at a temperature about 18° C. below that of the pure
metal. The presence of this material, which is of a blue colour when
viewed under the microscope, constituting slightly more fusible, tough,
non-conducting areas between the copper crystals, accounts for many of
the well-known effects of oxygen in metallic copper.
When oxygen is present in quantities above the eutectic proportion, the
first constituent to solidify from the molten over-oxygenated copper
is brittle copper oxide, and the presence of such brittle material
disseminated through the metal explains why “dry copper” cannot be
worked.
The effects of comparatively small quantities of oxygen are greatly
increased on account of the fact that one part of oxygen, when present
as cuprous oxide, yields a constituent in almost nine times as great
a proportion by weight alone, since Cu_{2}O : O :: 142 : 16 or 9 : 1;
whilst oxygen existing as oxide-eutectic is represented in the ratio
of nearly 30 : 1. The presence of excess of copper oxide in the metal
is particularly dangerous when copper is to undergo annealing in a
reducing atmosphere, since the reducing gases acting upon the oxides
at the crystal boundaries destroy them, thus tending to produce that
rottenness in the material which is so often encountered under such
circumstances.
The great value and importance of oxygen in copper lies in its property
of bringing the metal up to pitch as indicated above.
The effect of carbon on oxygenated copper was the subject of much
enquiry in early years. It was thought at one time that the influence
of carbon _per se_ in the copper was responsible for the beneficial
effects resulting from the melting of brittle “dry” copper with carbon,
but the work of Percy, since confirmed, showed that its sole action is
in the reduction of the injurious excess of oxide.
In addition to the specific influences of oxygen as just recorded,
and to its important physical effects with regard to the solubility
of gases, etc., oxygen in copper performs other valuable functions,
by forming with reduced impurities which are exceedingly dangerous,
oxygenated compounds more infusible and more insoluble; and this has
the effect of segregating or distributing such injurious impurities
into forms and positions much less harmful.
[Illustration: _a_ _b_
Fig. 6.—Microstructure of Copper containing Oxygen (_Heyn_).
_a._ Hypo-eutectic. _b._ Hyper-eutectic.
Oxygen 0·13 per cent. = 1·16 per cent. Cu_{2}O.
Oxygen 0·53 per cent. = 4·7 per cent. Cu_{2}O.]
[Illustration: Fig. 7.—Relations of Copper and Arsenic.]
_Arsenic in Copper._—When arsenic and copper are melted together
chemical combination occurs, and a series of arsenides is produced;
the system, which has been investigated by Friedrich (from whose work
the following diagram has been constructed), Hiorns, Bengough & Hill,
and others, being one of considerable complexity. With proportions of
arsenic such as are usually present in commercial coppers, the compound
produced is probably Cu_{3}As (28·3 per cent. of arsenic), which
passes into solution in the excess of metal, and on solidification the
copper retains this arsenide in solid solution. As in the case of all
such solid solutions, the solidification takes place over a range of
temperature represented between the liquidus and solidus curves; the
purer metal crystallising out first, followed gradually by crystals
of copper which become progressively richer and richer in arsenic
(still in solid solution). In the case in question, diffusion of the
arsenic throughout the crystalline mass proceeds but slowly, and as
a result, the metal, as usually obtained in the cast state, shows
fringes of such arsenic-rich copper. By annealing, diffusion is greatly
assisted, and the material gradually becomes homogeneous, as is seen
on microscopic examination. There appears further to be some decrease
of this solubility with fall of temperature when the arsenic is high,
leading sometimes to a separation of the arsenide itself at the crystal
boundaries.
_Antimony_ appears to form an analogous compound, Cu_{3}Sb, also
capable of passing into solid solution in the copper, but to a
rather smaller extent than the corresponding arsenide. The fringes
are therefore more pronounced, and the decrease of the solubility on
further cooling is also more marked.
_Bismuth._—The influence of even minute quantities of bismuth on
copper is notorious. Bismuth appears to be soluble in liquid copper,
but not in the solid metal. In consequence, when copper containing
bismuth solidifies, the copper crystals separate first, whilst the
liquid bismuth still remains between them, until the metal reaches a
temperature of about 268° C.—the melting point of bismuth—when it too
solidifies _in situ_. The presence of such envelopes of very brittle,
fusible, and limpid bismuth material explains much of the harmful
effect of this impurity. These envelopes are found to consist almost
entirely of practically pure bismuth. Oxygen converts the bismuth into
a more compactly crystalline oxide, much less fusible and harmful.
Arsenical copper tends to the scattering of the bismuth globules
among the fringes which are formed during the gradual process of
solidification over the range of temperature already indicated, and
thus renders this impurity to some extent less dangerous.
_Lead_ behaves in apparently much the same way as bismuth, and the
effects produced upon it by the presence of oxygen and arsenic are
probably similar.
_Selenium and Tellurium_ probably exist in the form of selenides
and tellurides, which are characterised by marked brittleness and
fusibility.
=Mechanical Properties of Copper.=—The mechanical properties of
commercial copper are influenced to a vital degree by the conditions
associated with working practice, such as composition, previous
mechanical and thermal treatment, temperature of working, etc. As has
been already indicated, it is the possession by the copper of certain
mechanical qualifications which leads to its employment by engineers,
and it is, therefore, necessary to consider the influence of the above
conditions, when reviewing the mechanical properties of the metal.
Much of the copper employed for general engineering work (apart from
electrical and alloying purposes) is of the quality designated as
“tough-pitch” copper. This tough copper generally contains certain
impurities which render the metal exceedingly useful for mechanical
service, and their presence is, indeed, almost essential in copper
intended for such purposes. At the same time, such elements would
render it absolutely unfit for the other uses just specified, where
purity is practically the first necessity.
The standard works and the papers indicated in the appended list of
references should be consulted for details concerning the effect of
each circumstance on the several mechanical properties; certain general
considerations must, however, be noted here.
Not only should the composition of the metal be carefully considered,
but attention must be directed to the actual condition and distribution
of each constituent. Owing largely to the difficulties of determining
the oxygen contents in copper, and to a want of definite knowledge as
to the condition, amount, and effects of the dissolved gases in the
metal, the information at present available is not sufficiently concise
to allow of a systematised statement being made as to the direct
influence of the constituents on the mechanical properties. This is
more especially the case since the other attendant circumstances of
working practice may react through these to a considerable extent.
Many of the more general results have, however, long been known to
engineers from practical working, and these have been placed on record
from time to time.
The _malleability_ and _ductility_ of copper are considerable. Cold
rolling and hammering causes a reduction in this respect, and the
metal is hardened, but the properties are restored by annealing.
The annealing effect commences at about 300° C., but proceeds
more effectively at higher temperatures, the factors of annealing
temperature and duration necessary for annealing being inversely
connected. The impurities which influence these properties most
adversely are bismuth and tellurium. The effect of other constituents,
oxygen _per se_, sulphur, and iron, in the quantities usually present
in commercial copper, is very small. Arsenic and antimony up to 0·4
or 0·5 per cent. have no deleterious effect on the malleability and
ductility of copper _of the correct pitch_, and may even improve the
metal when tested in the cold; the hot malleability is, however,
somewhat decreased.
The presence of impurities raises the temperature required to
bring about the full effects of annealing after the metal has been
hardened by mechanical work. This action is probably explained by
the interference of the impurities upon the molecular freedom of the
metal, which controls the mechanism of annealing. The conditions,
whether reducing or oxidising, during annealing, may exert an important
influence on the results.
_Hardness._—Pure copper is a comparatively soft metal. It is hardened
by mechanical work—the hardness of rolled copper, determined by the
Brinell Test, being 74 compared with mild steel as 100—and by the
presence of even small quantities of impurities, tin possessing a
particularly marked effect in this connection. The worked metal is
softened on annealing.
_Tensile Strength and Elongation._—The strength of copper, being a
property of such practical importance, has been the subject of much
extended investigation. The work has, however, been conducted under
such a great variety of conditions, many of which have been left
unrecorded, that co-ordination of the results is barely possible,
and does not allow of establishing on a definite basis the effect of
different influences on this property of the metal. Later work, some
already published, some still in progress, should eventually allow
of more general standardisation than is at present possible. The
tensile strength of pure cast copper is 8 to 9 tons per square inch.
Mechanical work causes an increase in the value up to 14, or even 16
tons, cold work exerting a still more marked influence; whilst 33 tons
and more per square inch has been recorded with cold-drawn fine wire.
The elongation varies according to the mechanical work which the metal
has undergone; the amount ranges from 35 to 40 per cent. and upwards,
measured on a 3-inch length.
Tensile strength is reduced on annealing, but never to so low a
degree as that of the cast material, the usual figure being 12 to 14
tons per square inch. The effect of temperature in reducing tensile
strength, especially when impurities are present, is important from the
industrial point of view. The reduction in strength caused by annealing
appears to be considerably smaller in the presence of arsenic and
antimony.
Arsenic increases the tensile strength of copper when the metal
is of the correct pitch, generally to well over 15 or 16 tons,
in the presence of the proportions usually found. Antimony has a
similar effect. Some workers state that, within certain limits, the
strengthening effect of this element is even more pronounced. Excess
of antimony exerts, however, a much more adverse influence than does
excess of arsenic. The elongation is increased by the presence of
moderate quantities of arsenic.
Oxygen _per se_, when present in moderate quantity in copper, has but
little effect on the tenacity. Bismuth, tellurium, sulphur, and lead
are the impurities which lower the strength, even when present in
minute quantities, and especially on heating. Bismuth in the proportion
of 0·005 per cent. lowers the malleability and ductility considerably,
and recent reports state that 0·02 per cent. bismuth renders copper
cold short, that 0·05 per cent. makes it red short, and that 0·005
per cent. is the limit for electrolytic copper which is to be rolled.
The deleterious effects of bismuth are, as already explained, to some
extent masked by the presence of arsenic and by oxygen.
The strength is increased by the presence of nickel, tin, and zinc in
the proportions usually present in the commercial metal; these are,
however, generally small.
From the foregoing review, indications will be afforded of the reasons
for the choice by engineers of “tough-pitch” copper for much of their
work, and the explanation for the 0·3 to 0·5 per cent. arsenic often
particularly specified for. The frequent use of arsenical coppers for
such purposes as fire-box plates will also be understood, since the
arsenic not only improves the mechanical properties of the metal, but
ensures the retention of rigidity and strength at the high working
temperatures required, to a greater degree than would have been the
case had pure copper been employed.
The effect of the above factors on the elastic limit of copper, is
also very marked and of much importance, the influence being closely
analogous to that produced on the other mechanical properties.
=Chemical Properties.=—The atomic weight of copper is 63·57. The metal
is unchanged in dry air at ordinary temperatures; in the presence of
moisture and of carbon dioxide a green coating of basic carbonate is
produced. When heated in air, a black scale, consisting of cuprous
oxide, Cu_{2}O, is obtained, which is readily detached by quenching
and hammering. Water at ordinary temperatures is without effect upon
copper; concentrated sulphuric and nitric acids have little action
upon it in the cold, but attack it on heating. The best solvent for
the metal is dilute nitric acid, which dissolves it very readily.
Copper is liable to corrosion when subjected, whilst hot, to the
action of chlorine or hydrochloric acid gas; this action has provided
an explanation of the corrosion of copper boiler tubes where the coal
employed had been exposed to sea water.
Copper is deposited from solution as a dull red, spongy mass, by iron,
zinc, or aluminium, but it is more electro-positive than gold or
silver, and readily precipitates these metals from solutions of their
salts, these effects being extensively made use of in practice. The
metal possesses a powerful affinity for sulphur, and this property has
very important applications in the smelting processes.
Copper readily alloys with gold, silver, tin, zinc, and nickel, but not
with lead or iron.
References.
Composition and Properties of Metal for Railway and Locomotive Work
(p. 20).
_Proc. Inst. Mech. Eng._, 1893; Dean, p. 139; Blount, p. 164;
Watson, p. 168; Gowland, p. 176; Aspinall, p. 193;
Tomlinson, p. 182.
Webb, F. W., “Locomotive Fire-box Stays.” _Proc. Inst. C.E._, 1902.
Milton, J. T., “The Treatment of Copper for Steam Pipes.”
_Inst. Marine Eng._, 1908–9.
Hughes, G., “Non-ferrous Metals in Railway Work.”
_J. Inst. Metals_, Sept. 1911.
Law, E. F, “Alloys.”
Influence of Impurities on the Electrical Conductivity of Copper
(p. 24).
Lawrence Addicks,
_Trans. Amer. Inst. Elect. Eng._, 1903, vol. xxii., pp. 695–702;
_Electro-Chemical Industry_, 1902–3, pp. 580–583;
_Trans. Amer. Inst. Min. Eng._, 1906, vol. xxxvi., p. 18.
Walker, A. L., _Mineral Industry_, 1898, vol. vii., p. 248.
T. Johnson, “Some Features in the Metallurgy of Copper.”
_Proc. B’ham. Met. Soc._, 1906.
Hiorns and Lamb, “Influence of Arsenic and Antimony on Copper.”
_Journ. Soc. Chem. Ind._, May, 1909.
Condition and Influence of Impurities on the Mechanical Properties
of Copper (p. 32).
┌─
│ _Zeitschrift für Berg. Hutten and Sal. Wesen_,
Hampe ─┤ 1873, xxi., 218; 1876, xxiv., 26
│ _Chemiker Zeitung_, 1892, No. 42, p. 16.
└─
┌─
Heyn, E., │ _Reports, Royal Tech. Testing Institute._
“Copper and Oxygen.” ─┤ Charlottenburg, 1900, p. 315.
│ _Metallographist_, vol. vi., 1902, p. 48.
└─
Arnold, _Engineering_, vol. lxi., p. 176. Feb. 7, 1896.
Roberts-Austen, Second Report, Alloys, Research Committee.
_Proc. Inst. Mech. Eng._, April, 1893, p. 114.
Rudeloff, _Mittheil. König. Tech. Versuchs. Anstalt._, 1894, ii.
(_b_), pp. 292–330; 1898. 16_a_, pp. 171–219.
Lawrie, _Bull. Amer. Inst. Min. Eng._, 1909, pp. 857–66.
“Bismuth in Wire Bar Copper.”
Johnson, F., “Impurities in Tough Pitch Copper containing Arsenic.”
_Proc. Inst. of Metals_, 1910, vol. iv.; No. 2, p. 163, _et seq._
Johnson, F., “The Influence of Impurities on the Properties of
Copper.” _Metallurgical and Chemical Engineering_, Oct. 1910,
p. 570.
“Annealing of Copper and Diseases of Copper.” _Ibid._,
Feb. 1911, p. 87.
“Notes on the Metallurgy of Wrought Copper.” _Ibid._,
August, 1911, p. 396.
See also Standard Specifications for Copper Wire-Bars (recommendations
by the Committee of the American Society for Testing Materials). _Eng.
and Min. Journ._, Jan. 20, 1912, p. 181.
LECTURE III.
Compounds of Copper — Copper Mattes — The Varieties of
Commercial Copper — Ores of Copper — Preliminary
Treatment of Ores, Sampling.
=Compounds of Copper.=—From the smelting point of view, the three most
important classes of copper compounds are the oxides, the sulphides,
and the silicates.
_Copper Oxides._—Of the oxides, two are of importance—cuprous oxide,
Cu_{2}O, and cupric oxide, CuO—the first-named particularly, having
extensive connection with smelting practice.
Cuprous oxide is black when in the massive form, and has a red hematite
colour when powdered. It is readily formed by the oxidation of copper,
and melts at a red heat without decomposition; further heating in the
presence of air produces the cupric oxide which is less fusible. As has
been already indicated, cuprous oxide dissolves in the molten metal. It
is easily reduced to metallic copper by heating with carbon, the metal
being also obtained if the oxide be heated in the presence of reducing
gases; it combines readily with silica when heated, yielding fusible
silicates.
When cuprous oxide is heated with sulphide of iron, the copper, having
a greater affinity for the sulphur than iron possesses, enters into
combination with it, forming copper sulphide and iron oxide, and if
sufficient silica be present, a silicate of iron slag is produced. When
melted with copper sulphide, cuprous oxide yields metallic copper with
liberation of sulphur dioxide according to the equation—
Cu_{2}S + 2Cu_{2}O ➡ 6Cu + SO_{2}.
This reaction is a quantitative one, and takes place in the Direct
Process of Nicholl and James as operated at Swansea. The excess
of either constituent remains unchanged. The reaction is of great
importance in the processes of copper extraction, since upon it depends
the liberation of metallic copper from the sulphide, both in the old
roaster process and in the modern converter operation.
_Sulphides of Copper._—Of the sulphides Cu_{2}S and CuS, the former
only is of metallurgical importance. It is grey black, brittle, and
crystalline, its melting point is about 1,135° C., and its specific
gravity, when cold, about 5·5. Owing to the great affinity of sulphur
for copper, this element acts as practically the universal carrier of
the metal in smelting work, detaching the copper from all other forms
of combination, and collecting it as sulphide, mixed with the sulphides
of other metals, particularly that of iron—copper sulphide and iron
sulphide alloying in all proportions.
When copper sulphide is melted with an excess of sulphur, it remains
unchanged; when melted with copper and subsequently cooled, the
sulphide and metal separate as such, although it is believed that
small amounts of copper are present in solid solution in the sulphide
on solidification, but that they separate from it during a dimorphic
change in the material, which occurs at about 103° C. The sulphide
reacts with iron with liberation of some metallic copper, and the
formation of some iron sulphide which associates itself with the rest
of the copper sulphide, forming a matte. This matte is not further
affected by iron, so that it is not possible to completely decompose
copper sulphide by this means.
When heated in a powdered condition in excess of air, copper sulphide
is oxidised, oxides of copper and sulphur being produced. There occur
probably several intermediate reactions, and several intermediate
products are formed, but the main effect is represented by the
equations—
┌─
│ Cu_{2}S + 2O ➡ 2Cu + SO_{2}
─┤
│ 2Cu + O ➡ Cu_{2}O
└─
which take place simultaneously, the copper represented in the first
equation being oxidised spontaneously according to the second, and the
resultant is the reaction Cu_{2}S + 3O ➡ Cu_{2}O + SO_{2}.
In the furnace operations, some of the SO_{2} in the presence of air
and oxidisable material, and in contact with the heated brickwork
becomes oxidised to SO_{3}, which, interacting with the oxides and
sulphides present, combines to form copper sulphate and cupric oxide.
At a higher temperature the sulphate is again decomposed to CuO and
SO_{3}, some of which passes off and is free to oxidise more sulphide;
the rest is decomposed to SO_{2} and oxygen. These reactions occur
during the roasting of charges containing copper sulphides.
=Copper Mattes.=—On smelting a furnace charge which contains both
copper and sulphur, the sulphur appears to have a stronger attraction
for the copper than for any of the other metals usually present, and
only when this affinity has been satisfied is the excess sulphur free
to combine with other constituents of the charge. The fusible copper
sulphide which is thus produced, has the power of mixing completely
with any more sulphides which may be present, especially with sulphide
of iron.
The fused sulphides resulting from such furnace operations are termed
_copper-mattes_. They may contain from a mere trace to upwards of 80
per cent. of copper, and in ordinary work, sulphide of iron is the
other constituent present in the greatest proportion, but sulphides
of nickel, silver, zinc, or lead, etc., may also be found, as well as
arsenides and antimonides.
These facts relating to the collection of the copper as a constituent
of a fused sulphide product, form the basis of modern copper-smelting
work. In view of the practical importance of the mixed sulphides,
the diagram representing their equilibrium requires notice. A number
of workers have studied the question with widely differing results.
Röntgen made an exhaustive investigation of the system FeS—Cu_{2}S, and
published a very complete diagram of the series, working with FeS and
Cu_{2}S in the pure state.
The sulphides as commonly met with, especially in smelting practice,
do not however, occur as materials of the composition denoted by
the formulæ Cu_{2}S and FeS. The ordinary commercial sulphide of iron
corresponds more closely to the impure eutectic of the iron-FeS
system, containing about 85 per cent. of FeS and 15 per cent. of
iron, and melts at about 970° C., whereas the pure FeS has a melting
point of upwards of 1,180° C. At the elevated temperatures of the
copper-smelting furnace, pure FeS tends to lose sulphur and to assume
the composition of the eutectic. There are, further, good reasons for
believing that copper sulphide behaves in a somewhat similar manner, so
that the series of sulphides constituting the mattes of practice are
not represented by pure materials so well as by a series composed of
mixtures of the respective eutectics.
The diagram of this series of industrial sulphides was worked out by
Hofman, Caypless, and Harrington, and gives a fair summary of the
melting points of the series of mattes. It is reproduced in fig. 8. The
temperatures may be supplemented by Gibb’s determinations of 1,121° C.
for the 71·7 per cent. copper matte, and 1,098° C. for the 80 per cent.
matte.
The problem of the constitution of mattes is, however, a very complex
one, and is not yet satisfactory settled. An interesting view was put
forward by Gibb and Philp. Mattes corresponding to the formula 5Cu_{2}S
. FeS (copper 71·7 per cent.), when examined microscopically, appeared
to be homogeneous, and indicated some form of combination between
the sulphides in these proportions. Lower-grade mattes were assumed
to consist of this compound substance and excess FeS. Iron sulphide
was held to be capable of carrying a certain quantity of copper in
solution, and mattes might, therefore, carry this copper, according to
the amount of excess FeS which they contained. Within certain limits
the lower the grade of the matte—_i.e._, the more FeS present—the
more copper was held in solution, and with a fall of temperature this
solubility was lessened, and moss copper was set free in the solid
matte.
[Illustration: Fig. 8.—Freezing-Point Curve of Iron-Copper Sulphides
(Mattes).]
Deposition of copper may also be accounted for by a variation in the
solubility for copper, accompanying the well-marked dimorphic change
occurring in FeS at 130° C. whilst another possible cause of the
separation of moss copper is the partial decomposition of Cu_{2}S,
being effected, as previously indicated, by the free iron of the
iron-FeS eutectic which constitutes the iron sulphide component of
copper mattes. The whole subject is thus of considerable complexity,
and involves questions of thermal and chemical equilibrium.
The appearance, chemical constitution, and physical properties
of mattes vary according to the rate of cooling, and are further
influenced by the nature and amount of the impurities they contain,
and the following statement must be understood to be more or less
general:—Usually low-grade mattes (up to 20 per cent. or so of copper)
are more or less stony in fracture, with a bluish-purple colour; as the
copper contents increase, a reddening of the colour occurs, and also
an increase in the crystalline character and brittleness. Considerable
quantities of moss copper are present in these mattes. Beyond 30 per
cent. of copper, increased softness and brittleness result, with a
darkening towards blue-black in the colour, whilst with the 60 to 70
per cent. mattes the colour becomes in general of a steel-grey hue.
Increase in the copper contents leads to an increase in the density—a
matter which has important applications in connection with the
economical separation of matte from slag, and the slag-losses in
smelting practice.
The specific gravity of the 13 per cent. copper matte is about 4·80.
" 43 " " " 5·18.
" 60 " " " 5·42.
" 80 " " " 5·55.
(_Gibb_ and _Philp_.)
The density in the fluid state, which is the important condition in
smelting, is less than this, and may indeed be somewhat different,
owing to changes in the constitution of the material.
_Copper Silicate_ is formed by the action of copper oxide and silica
on heating. The silicate is decomposed when heated in the presence
of sulphides, resulting in the formation of sulphide of copper and
silicate of the second metal, in consequence of the great affinity of
copper and sulphur. Upon this fact depends the extraction of copper
from various silicate ores, as well as the cleaning of slags high in
copper, which are often added to the sulphide charges in the furnace
with this object. When heated with iron, the silicate is reduced to
metallic copper with the production of silicate of iron; it is also
reduced by carbon in the presence of metallic oxides capable of uniting
with the silica which is liberated.
=The Varieties of Commercial Copper.=—The copper employed industrially
comes into the market in widely differing forms. Different varieties
are named according to the method of manufacture, the uses for which
they are intended, the locality in which they are produced, or by
special trade names. The most important variety is:—
_Electrolytically-refined High-conductivity Copper_, which is largely
used for electrical work. The methods by which it is produced ensure
that most of the impurities inimical to high conductivity have been
removed, and the metal is specially free from arsenic, antimony, and
bismuth, as well as from silver and gold. As ordinarily produced
at the electrolytic refinery, it is in the form of cathode plates,
often about 3 feet × 2 feet 6 inches by ¾ inch thick, weighing 150
to 170 lbs. It is then remelted in order to bring it “up to pitch,”
and to give it the necessary mechanical properties, so that it may
be transformed at once into the particular form suitable for the
electrical purposes intended. Such metal often comes into the market in
the form of wire-bar ingots, cakes, or billets, weighing from 70 to 500
lbs. when in bar form, and from 100 to 400 lbs. when in other shapes.
Electrolytic copper is also suitable for the manufacture of alloys.
_Lake Copper._—The copper ores of the Lake Superior district are
particularly pure, and on smelting and furnace-refining yield a
metallic product of great purity which also possesses good mechanical
properties. It is, therefore, particularly suitable for electrical
work. By reason of its satisfactory properties, Lake copper realises
prices which usually rule somewhat higher than those of ordinary
electrolytic copper as quoted on the New York market.
_Best Select Copper._—For the production of copper alloys, such as
best brass, etc., it is essential that the copper should be pure.
The impurities which are present in ordinary tough copper, and which
may be valuable for imparting strength to the material, have a very
harmful effect when present in alloys. In the older Welsh process of
manufacturing copper, a special method was employed for obtaining metal
free from these impurities, especially arsenic and antimony. This was
known as the “best selecting” process.
The principle underlying the method was to conduct the furnace
operations to the stage at which a small quantity of copper, known as
“copper bottoms,” was obtained. The metal so produced has the property
of collecting from the rest of the matte-charge in the furnace, the
gold, the silver, and the great bulk of the other impurities, owing
to its greater solvent power for them. As a result, the greater part
of the matte (“white metal”) was left pure, and from this material
the copper was extracted by continuing the furnace operations in the
usual manner, the resulting product being known as “best select” (B.S.)
copper.
The process was later used principally for the extraction of the gold
in the charge, rather than for obtaining specially pure copper. The
product is essentially a British one, and was largely used for the
manufacture of high quality alloys.
“_Tough Pitch Copper._”—The operation of “bringing copper up to pitch”
has for its object the imparting to the metal of the toughness and
mechanical strength required for industrial service. The process
resolves itself into the adjustment of the correct proportion of
oxygen, the function of which is largely to eliminate the gases from
the copper, or to overcome their deleterious effects, as well as to
convert the otherwise more injurious metalloid impurities into a less
harmful form.
In modern practice, practically all copper is brought up to pitch, but
it is useful to distinguish between tough-pitch furnace-refined copper
and tough-pitch electrolytic copper.
The former is the brand to which the general term “tough pitch
copper” is best applied, this name having been given to the product
from the refining furnaces of the old Welsh and similar processes.
Before the converter method was introduced into copper practice,
the furnace processes for extracting copper from the ores resulted
in the production of a crude “blister” copper, into which several
injurious constituents, if originally present in the ore, found their
way. The principal impurity was usually arsenic. Although this was
also removable by special refining methods, and with some difficulty,
it was known, as has been indicated, that when arsenic is present
under suitable conditions and in proper proportions, it is capable of
imparting considerable strength and rigidity to the metal. Such copper
being particularly suited for various engineering and mechanical uses,
the arsenic being sometimes even specified for and purposely added—as
in fire-box plates and stay bolts, though it is never employed for
conductivity work or for the manufacture of alloys if any considerable
proportion be present—the metal found a ready market when brought to
pitch.
Tough pitch copper may thus vary largely in composition, especially
in arsenical contents, up to about the 0·5 per cent. already
indicated as being mechanically very useful. The actual process, as
used for bringing all classes of metal to pitch, will be described
in detail later, it being practically the same whether conducted on
furnace-refined metal, converter metal, or on electrolytic copper, as
a necessary preliminary to casting into the various forms of ingot in
which it is to be marketed.
In preparing the tough metal from crude copper, the more oxidisable
impurities (iron, sulphur, etc.) are first removed by a thorough
oxidation during or after melting down, this being known as “airing.”
The operation oxidises some of the copper, and it is probable that the
copper oxide thus formed plays an important part in getting rid of
impurities. By the time they have been thoroughly expelled, the metal
is considerably over-oxidised. Samples taken at this stage exhibit
the following characteristics:—The ingot has a depression down the
centre line, the material is very brittle, the fracture is brick-like
in texture and purple-red in colour, whilst much copper oxide and
oxidule-eutectic are seen on examination under the microscope. This
material is known as _Dry Copper_; it is merely an intermediate
product, and is commercially useless. The excess of oxygen is removed
by “poling”—that is, reduction, effected largely by charcoal, as well
as by reducing gases—successive samples showing less and less of the
characteristics of dry copper. The surface becomes level, the metal
exceedingly tough, the fracture fine-grained to silky in texture, and
a fine salmon-pink in colour. With satisfactory mechanical properties,
the metal has now become =tough pitch copper=.
If the poling—that is, the reduction of the oxidised constituents of
the tough pitch copper—be carried too far, the metal becomes brittle
again, being known as _over-poled copper_. The fracture then tends to
become coarse and fibrous, the colour lighter, and the upper surface
of the ingot exhibits a ridge. The reasons for these effects have not
yet been quite fully explained, but there is no doubt that they arise
from the removal of oxygen from the oxygenated constituents, and the
withdrawal from the metal of the protecting influence of the cuprous
oxide. Such influences are to some extent physical, since they prevent
the retention of the reducing gases; partly mechanical, in their
effects on the properties of the metal _per se_, and partly chemical,
as the oxide had probably entered into chemical combination with some
of the objectionable impurities, producing compounds, in which form
they were much less harmful. The removal of this oxygen from the metal
breaks down such combinations, leaving the reduced impurity again to
exercise its destructive effects on the properties. Over-poled copper,
like dry copper, being brittle, is commercially useless as such, and is
really an intermediate product, the metal being brought to pitch again
by further aëration to make it “dry,” after which it may be poled back
to correct pitch. As already stated, the over-poling effects are not
due to any intrinsic action of carbon directly on the copper itself.
Summarising, it may be stated that the most important commercial
varieties of copper are:—
=Electrolytically-refined metal=, employed for electrical work (also
for alloy-making).
=Tough Pitch Copper= for engineering uses.
=Best Select Copper= for alloy manufacture.
And, in addition, Lake Copper and some Converter Bars.
A number of unrefined metallic products met with in practice include:—
_Converter Bars._—The product from the Bessemer operation on copper
mattes. Most converter metal is subsequently electrolytically refined,
but several varieties of Australian and American copper are put on
the market direct in this form. Being produced from fairly pure ores,
which carry but little silver and gold, the converter metal may be
sufficiently pure to render electrolytic refining unnecessary, and too
low in gold and silver values to make such an operation profitable.
_Cathode Copper_ is the product from the electrolytic refinery, and is
usually remelted, brought up to pitch, and cast into ingots previous to
use.
_Black Copper_ is produced by the smelting of oxide ores, and is
subsequently refined.
_Cement Copper_ is produced by wet processes, usually by precipitation
from copper-bearing solutions by means of iron, the product being
a rather impure reddish-brown spongy mass. Many varieties contain
arsenic. It requires melting and subsequent refining to adapt it for
service.
_Blister Copper_ was the name given to the crude metal from the older
type of furnace operations. Such copper contained large quantities
of gas, particularly SO_{2}, which, tending to escape at the moment
of solidification in the mould, gave a blistered appearance to the
surface. It contained 96 to 98 per cent. of metallic copper, and was
subsequently refined. The term is generally applied still to all crude
copper exhibiting similar features.
_Chili Bar_ is an impure copper imported from Chili for refining. The
composition varies, the metal usually containing 96 to 98 per cent. of
copper, with indefinite quantities, sometimes small, of undesirable
impurities.
Appended is a series of representative analyses of various copper
products, compiled from different sources. The composition of such
material as tough pitch copper and the various cruder varieties is,
however, subject to very great variation.
=The Sources of Copper.=—Copper ores usually consist of various
minerals of copper mixed with those of many other metals, and
accompanied by very varied gangue, according to the locality in which
they are found.
They are best classified under three groups:—
(1) _Native Ores._
(2) _Sulphide Ores._
(3) _Oxide Ores._
The most important points to be noted with regard to the distribution
of these different classes are that—
(1) Native ores are localised in their occurrence, being chiefly
confined to the Lake Superior district.
TABLE IV.—ANALYSES OF VARIOUS COMMERCIAL COPPERS.
──────────────────────────────┬───────┬──────┬───────┬───────
│Copper │ Gold │Silver │ Lead
──────────────────────────────┼───────┼──────┼───────┼───────
1. Electrolytic conductivity │ 99·89 │ nil │ nil │ nil
copper, │ │ │ │
2. Lake copper, │ 99·77 │ nil │0·029 │ nil
3. Best select copper, │ 99·75 │ .. │ .. │0·024
4. Tough pitch copper, │ 99·41 │ .. │ .. │0·070
│ 99·25 │ .. │0·36 │0·0103
5. Copper fire-box plate (ran │ │ │ │
500,000 miles, Met. Ry.),│ 98·70 │0·0001│0·0346 │0·4085
│ │ │ │
INTERMEDIATE PRODUCTS— │ │ │ │
Refined converter copper, │ 99·25 │ .. │0·36 │0·0103
│ 99·08 │ .. │0·30 │0·0085
Cathode copper, │ .. │ .. │0·001 │0·00054
Black copper, │ 94·39 │ .. │0·11 │0·19
│ 97·70 │ .. │0·2133 │0·78
Cement copper (Spanish), │ 51·90 │ .. │2·35 │1·45
│ 76·93 │0·10 │ .. │ trace
Blister copper, │ .. │0·0009│0·04 │0·042
Chili bar, │ 98·60 │ .. │ .. │ trace
──────────────────────────────┴───────┴──────┴───────┴───────
──────────────────────────────┬─────────┬────────┬────────┬───────
│ Arsenic │Antimony│ Bismuth│ Iron
──────────────────────────────┼─────────┼────────┼────────┼───────
1. Electrolytic conductivity │ 0·016 │ trace │ nil │0·042
copper, │ │ │ │
2. Lake copper, │ nil │ trace │ nil │0·0077
3. Best select copper, │ 0·025 │ trace │ 0·011 │0·10
4. Tough pitch copper, │ 0·320 │ trace │ 0·010 │0·010
│ 0·0211 │ 0·630 │ 0·0044 │ ..
5. Copper fire-box plate (ran │ │ │ │
500,000 miles, Met. Ry.),│ 0·3726 │ 0·0346 │ 0·0360 │0·0069
│ │ │ │
INTERMEDIATE PRODUCTS— │ │ │ │
Refined converter copper, │ 0·0211 │ 0·0630 │ 0·0044 │ ..
│ 0·0290 │ 0·0254 │ 0·0035 │ trace
Cathode copper, │ 0·00034 │ 0·0008 │ 0·0003 │ ..
Black copper, │ trace │ .. │ .. │ ..
│ 0·052 │ 0·2380 │ 0·0035 │0·17
Cement copper (Spanish), │ 2·95 │ 0·50 │ 0·95 │7·00
│ 1·32 │ 0·02 │ .. │7·6
Blister copper, │ 0·108 │ 0·157 │ 0·055 │0·4
Chili bar, │ 0·100 │ trace │ nil │0·009
──────────────────────────────┴─────────┴────────┴────────┴───────
──────────────────────────────┬────────┬────────┬────────┬───────
│ Nickel │ Tin │ Oxygen │ Sulphur
──────────────────────────────┼────────┼────────┼────────┼───────
1. Electrolytic conductivity │ 0·006 │ .. │ 0·008 │ nil
copper, │ │ │ │
2. Lake copper, │ 0·0146 │ nil │ 0·070 │ ..
3. Best select copper, │ 0·061 │ .. │ 0·143 │ ..
4. Tough pitch copper, │ 0·060 │ .. │ 0·120 │ ..
│ .. │ .. │ 0·284 │ ..
5. Copper fire-box plate (ran │ │ │ │
500,000 miles, Met. Ry.),│ 0·3039 │ .. │ 0·0181 │ 0·0064
│ │ │ │
INTERMEDIATE PRODUCTS— │ │ │ │
Refined converter copper, │ .. │ .. │ 0·284 │ ..
│ .. │ .. │ 0·12 │ 0·01
Cathode copper, │ .. │ .. │ 0·005 │ ..
Black copper, │ 2·04 │ 0·07 │ .. │ 0·80
│ .. │ .. │ .. │ 0·796
Cement copper (Spanish), │ .. │ .. │16·00 │ 5·10
│ .. │ .. │ .. │ 0·48
Blister copper, │ 0·0–0·2│ 0·0–0·5│ .. │ 0·112
Chili bar, │ .. │ .. │ .. │ 0·909
──────────────────────────────┴────────┴────────┴────────┴───────
(2) Sulphide ores supply the bulk of the world’s copper, constituting
upwards of 80 per cent. of the total.
(3) The oxidised ores are found in most copper districts, though
usually to only a limited extent. They are often gossan deposits
produced by weathering or by decomposition of sulphides, hence are
generally found nearer the surface, changing to sulphide with depth.
The supply of copper from oxidised ores, which was at one time very
large, is decreasing rapidly, and the greater proportion of the copper
now obtained from them comes from the more recently developed deposits,
of which those at Tanganyika afford an example.
More than 200 minerals which contain copper are known, but most of them
are unimportant from the smelting point of view. The characteristics of
the more noteworthy may be fully studied from text-books of economic
mineralogy.
=Copper Ores—Native Copper.=—Occurs extensively in the Lake Superior
district of Michigan, in Precambrian rocks, sparingly in New Mexico
and China, but seldom anywhere else in workable quantities by itself.
Copper barilla or copper sand, an impure native metal from Chili, was
formerly of importance. Native copper constitutes about 20 per cent. of
the North American supply. It yields metal of exceptional purity, and
the brands of Lake copper reach a very high standard, both as regards
electrical and mechanical properties. A still purer variety is the
native metal from Yunnan, China.
The Lake Superior copper occurs in three formations:—
(_a_) Vein deposits, from which the enormous masses of
copper are taken out.
(_b_) Copper-bearing ash beds, of amygdaloidal diabase.
Chief mine, Quincy.
(_c_) Beds of conglomerate in which the cementing material
consists partly of copper. This last class of deposits
yields three-quarters of the Lake copper supply. Their
average copper content is 2·9 per cent. The chief mines
are the Calumet and Hecla, the Tamarack and the Atlantic,
all situated on one ore chute measuring 3 miles in
length, and worked to a depth of 4,000 feet.
=Sulphide Ores=: _Chalcopyrite_ (_Copper Pyrites_) is by far the most
widely distributed ore of copper, and furnishes the greater proportion
of the world’s supply.
The formula when pure is Cu_{2}S. Fe_{2}S_{3} (Cu 34·4, Fe 30·5, and S
35·1 per cent.), but usually the ore is not in this condition, being
mechanically mixed with large quantities of iron pyrites, and very
often with pyrrhotite. It occurs principally in the older crystalline
rocks, often in bedded veins.
The value of copper veins below the limit of surface decomposition is
nearly always due to chalcopyrite. Silver and gold are often carried,
as well as other metals. It occurs extensively in Montana, Arizona,
Tennessee, Canada, Chili, Japan, Spain, Cornwall, etc.
Chalcopyrite ores vary considerably in copper contents; thus Tennessee
ores contain about 2·5 per cent. of copper, Montana ores 5 to 5½ per
cent. (with gold and silver valued at about £11 per ton of copper),
whilst the Arizona ores vary, being often rich.
_Chalcocite_ (also known as copper glance or redruthite) is much less
important. The copper contents are 79·8 per cent. when pure, but such
a condition is rare, although the ore seldom contains less than 50
per cent. of copper. Below this proportion it often tends to pass
into bornite, and then to chalcopyrite. It is found in Montana, is
an important ore in Arizona (Clifton district), and occurs also in
Cornwall.
Other important sulphides include:—
_Bornite_ (Erubescite, Peacock copper ore), 3Cu_{2}S.Fe_{2}S_{3},
occurring in Cornwall, which passes with depth into chalcopyrite.
_Tetrahedrite_ (Fahl ore), a very complex sulphide of copper, iron,
lead, zinc, with arsenic, etc. It is often rich, and carries silver
values.
=Oxidised Ores.=—The most important of the oxidised ores are—
_Malachite_, CuCO_{3}.Cu(OH)_{2}, containing, when pure, 57·3 per
cent. copper (73·7 CuO); is widely distributed, but usually occurs as
such in non-paying quantities except in a few particular localities. It
is found in the upper parts of the veins. Whenever found with sulphide
ores, it is an extremely useful material to mix in the charge, as it
supplies oxygen as well as copper. Malachite is still an important
source of the metal in Mexico, Chili, and Bolivia, though not quite so
much so as formerly, whilst it is specially important in the Tanganyika
(Katanga) deposits, of which it constitutes the greater portion so far
developed.
_Cuprite_, Cu_{2}O, contains 88·8 per cent. copper, when pure. It is
widely distributed, but is never found by itself in paying deposits,
though in the early days of mining and smelting it was an important
source of metal, since it was easily reduced, and consequently was
cheaply worked.
_Melaconite_, CuO, contains 79·8 per cent. copper, when pure; is fairly
widely distributed, although hardly ever in sufficient quantity to pay.
In one or two localities, however—viz., Tennessee, North Carolina, and
Virginia—it was formerly an important source of the metal. The deposits
were at first very promising, as they consisted largely of very rich
melaconite ore; this was however, quickly worked out, the ordinary
heavy chalcopyrite with 2·5 per cent. copper being struck below.
Other oxidised ores include—
_Azurite_, 2CuCO_{3}. Cu(OH)_{2}, and _Atacamite_, CuCl_{3}.
3Cu(OH)_{2}, from Chili.
In modern work, the chief ore smelted is impure chalcopyrite. Carbonate
and oxidised ores, when they can be obtained, are mixed with it,
increasing the concentration and shortening the process; except under
certain special circumstances.
=Preliminary Treatment of Ores.=—The treatment of ores preparatory
to smelting includes the processes of sampling, wet concentration,
agglomeration of fines, and roasting.
=Sampling.=—Since sampling is not a part of the extraction process
proper, in copper smelting, it will be convenient to deal with the
subject separately here.
It is important that ores and all other products entering or leaving
the works, as well as many of the intermediate products of the various
operations, should be properly sampled and assayed. Great attention
is paid to this point at the best organised smelters, since only by
this means can the work of the plant and of its several departments be
properly checked and controlled. Each works has its own special method
of taking samples from the stocks, the Anaconda practice, for example,
being to pass the whole of the first-class ore, amounting in quantity
to 25,000 tons per month, through the sampling mill, whilst of the
poorer, second-class, ore for concentrating, every fifth car-load is
sampled.
There are many different types of sampling plant, and the methods
employed vary also, but the principle is much the same in each
case—namely, to use some automatic device which cuts out and deflects
a certain proportion of the stream of ore on its course through the
mill;—the deflected portion being crushed finer, and a part of it again
cut out and deflected; repeating the operation in this way three or
four times.
The sampling process and plant at Anaconda is so representative of the
best practice, that it may be reviewed in brief, as an example.
[Illustration: Fig. 9.—Outline of Sampling Scheme, Anaconda.]
[Illustration: Fig. 10.—Section through Sampling Mill.]
The _Anaconda Sampling Plant_ is entirely automatic in its action.
The mill is built in two sections, each of which treats 1,800 tons
daily. Each section consists of a set of four sampling machines with
intermediate crushers. The ore goes from the bin to a Blake crusher,
breaking to 3-inch to 4-inch size; the crushed ore is elevated and fed
down a chute to the first sample cutter, which takes out one-fifth (400
lbs. per ton) as a sample, and deflects the rest down another chute.
The sample is crushed further in a Blake crusher, and passes a second
sample cutter (rather smaller in size), which again takes out one-fifth
(80 lbs. for every original ton of ore), and rejects the rest down the
“rejects-chute.” The sample is now crushed in rolls, a third cut of
one-fifth (16 lbs. of the ton) taken as before, the rest rejected. The
sample passes to a final set of crushing rolls, and the last cut of
one-fifth is taken. Hence each ton of ore is represented eventually by
3·2 lbs. of sample.
The sample cutter employed is of the Brunton form. It consists
essentially of a curved boat of 120° arc, which rotates to and fro on
a central spindle. The top is open; one side has one hole cut in, the
other has two, the area of the latter being together four times that
of the single one, so that the falling stream is cut continually, and
one-fifth is deflected to one side, falling down a chute to the next
crusher, whilst the other four-fifths fall from the other side to the
rejects-chute.
[Illustration: Fig. 11.—Brunton Sampler.]
The above description is quite general, several details for certain
classes of ore having been omitted, but it gives a fair idea of the
general principles underlying such work.
The final sample, say 3,200 lbs. per 1,000 tons of ore, is mixed on an
iron plate on the floor, quartered several times by a Brunton shovel,
and the chosen sample then ground in an Englehardt mill (small Gates’
crusher with two discharges). The material is passed through a 1-foot
riddle of 100 mesh wire cloth, the very small quantity of coarser stuff
remaining, is bucked down and added, and the whole is then thoroughly
mixed in a canister of 1 foot side gripped at opposite corners, and
rotated mechanically.
References.
_Constitution of Copper Mattes._
Keller. _Mineral Industry_, vol. ix., 1900, p. 240.
“Elimination of Impurities from Copper Mattes.”
Röntgen. _Metallurgie_, vol. iii., 1906, p. 479.
Hofman, Caypless, and Harrington.
_Trans. Amer. Inst. Min. Eng._, vol. xxxviii., 1908,
pp. 142–153.
Gibb and Philp. _Trans. Amer. Inst. Min. Eng._,
vol. xxxvi., 1906, p. 665.
Heyn and Bauer. _Metallurgie_, vol. iii., 1906, p. 84.
Fulton and Goodner. _Trans. Amer. Inst. Min. Eng._,
vol. xxxix., 1908, pp. 584–620.
_Refining of Copper._
H. O. Hofman, R. Hayden, and H. B. Hallowell,
“A Study in the Refining and Overpoling of Electrolytic Copper.”
_Trans. Inst. Amer. Min. Eng._
Hofman, Green, and Yerxa,
“A Laboratory Study of the Stages in Refining Copper.”
_Trans. Amer. Inst. Min. Eng._, 1904, vol. xxxiv.,
pp. 671–95.
Stahl, “Ueber Raffination, Analyse and Eigenschaften des
Kupfers.” _Berg. and Hüttenmännische Zeitung_,
1889, vol. xlviii., pp. 323–4; 1890, vol. xlix., p. 399;
1893, vol. lii., p. 19; 1901, vol. lx., pp. 77–79.
Keller. _Mineral Industry_, vol. vii., p. 245, _et seq._
_Sampling._
D. W. Brunton, “Modern Practice in Ore Sampling.”
_Mining and Scient. Press_, Oct. 30, 1909.
“Theory and Practice of Ore Sampling.”
_Trans. Amer. Inst. Min. Eng._, vol. xxv., p. 826.
LECTURE IV.
Modern Copper Smelting Practice — Preliminary Treatment
of Ores: Concentration, Briquetting, Sintering — The
Principles of Copper Smelting — Roasting.
=Modern Copper Smelting Practice.=—Until recently, modern smelting
practice has been understood to involve the production of a matte
containing from 40 to 50 per cent. of copper, which is then
bessemerised.
There are however proceeding at present (owing to the successful
working of basic-lined converters) developments which indicate that
such practice may, within a few years, be modified very considerably
in the direction of the converter treatment of lower-grade mattes.
Until such operations become successfully established and generally
adopted, the production and subsequent bessemerising of 40 to 50 per
cent. matte will be here dealt with as constituting modern practice;
particularly since, generally speaking, the principles involved are
equally applicable to the modified methods now being developed.
=Preliminary Treatment of the Ore.=—The factors which have to be
considered in drawing up a scheme of treatment for the supply of ores
shipped to a smelter are exceedingly numerous, and will be discussed in
due order. There are no hard and fast principles which determine such
schemes, yet a number of considerations must be noted concerning the
treatment preliminary to the actual smelting of the ores.
Such preliminary treatment may include—
_A. Concentration or Wet Dressing._
_B. Agglomeration of Fines—(a) Briquetting, (b) Sintering._
_C. Roasting._
_A._ =Concentration or Wet Dressing.=—In treating the ores of copper,
it may be noted that in general—
_Native Ores_, unless very massive, are usually dressed in a special
manner peculiar to themselves—_e.g._, stamp-milling.
_Oxide Ores_ are rarely wet-dressed. They present much difficulty in
treatment on account of their comparatively low density, which makes
efficient wet concentration almost impossible, whilst heavy losses in
the tailings generally accompany such operations.
_Sulphide Ores._—No definite rules can be laid down as to whether the
ore should be wet-dressed or not; the treatment depends altogether
on attendant circumstances, such as—(_a_) the character of the ore,
(_b_) the concentration of the copper desired in the first smelting
operation, and (_c_) the smelting method and furnaces adopted.
Wet concentration is only profitable when the copper ore is of low
grade, and then only under suitable conditions. Thus the low tenor
may be due to admixture with much gangue or with other sulphides, or
both. A massive low-grade pyritic ore carrying but little gangue is
not suitable for such treatment, since the mixed sulphides are not
separated from one another by wet dressing, and consequently but little
enrichment of the copper in the dressed product would be possible;
apart altogether from other considerations. Such is the case, for
instance, with the Tennessee ores carrying about 2·0 per cent. of
copper and only 25 to 35 per cent. of gangue.
An ore with a self-fluxing or almost self-fluxing gangue might allow of
its copper being concentrated more cheaply and conveniently by direct
smelting than by wet dressing, this depending, of course, on the local
conditions.
In other cases a balance has to be struck as to whether the
circumstances are more favourable for removing the excess of gangue by
means of crushing and treatment in a stream of water, or by slagging it
off in a furnace with the addition of suitable fluxes. In many cases,
with low-grade ores, the former treatment is the cheaper.
The case of the low-grade ores of the Butte, Montana, district, affords
a good example of these considerations. This ore contains 5 to 5½ per
cent. copper, with a large quantity of highly siliceous gangue. It
was found that the purchase and carriage of sufficient flux, and the
cost of carrying out this fluxing operation was so expensive that it
was cheaper to build a concentrator and smelter at Anaconda, 30 miles
away—in a locality where a suitable water supply was available for the
dressing—and to convey the ore this distance in order to concentrate it
by a wet method. The dressed ore assays 9 to 10 per cent. of copper.
It is important to note that the process of wet dressing involves
crushing the ore, and yields the product in a more or less finely
divided form. Most copper sulphide minerals are exceedingly brittle,
and break up to a very small size on crushing for concentration, so
that the copper concentrates usually include a large quantity of fine
material.
There are two general types of furnace available for
smelting—reverberatory furnaces and blast furnaces—and the questions
of the desirability and of the degree of crushing and concentration
depend to a large extent on the plant and furnaces adopted or proposed.
Blast-furnace treatment has hitherto often been considered the most
economical process for smelting copper ores, especially with regard to
fuel costs, but for many reasons it is not a convenient or efficient
furnace for the direct treatment of fine material. When it is desired
to employ the blast furnace, it is necessary to make up charges
consisting, to as great an extent as possible, of coarse material.
In consequence, when concentrating ores with a view to subsequent
blast-furnace treatment, the degree of crushing and dressing has to be
modified with these factors in view; otherwise a further preliminary
manipulation of the fine concentrates that are produced is rendered
necessary. Such modified dressing schemes involve a maximum of coarse
breaking and screening, the crushing and separating stages being thus
very gradual, and the units in the plant are multiplied, whilst the
process is rendered complex in consequence. With the greatest care,
moreover, large quantities of fines are bound to be produced, and have
to be dealt with by some means other than immediate blast-furnace
treatment.
Dressing schemes and plant for sulphide copper ores are thus often
complicated, particularly for the recovery of the values from the finer
material, and cannot be discussed at any length here. Reference should
be made to Richards or other standard works on the subject.
As representative of wet-dressing practice, the Anaconda scheme may be
noted, as summarised below.
There are eight mills, each treating 1,000 tons of ore per day, and
conducting the—
Coarse crushing in Blake crushers.
Coarse sizing by trommels.
Coarse separation on Harz jigs of 1¼-inch and ⅞-inch feed.
Middlings crushing in rolls.
Middlings sizing by trommels.
Middlings separation on fine jigs of 7, 5, 2½, 1½, and
1 millimetre feed.
Finest crushing in Huntingdon mills.
Fines settling by spigot settlers.
Fines separation on Wilfley tables (471 are in use on the plant).
The muddy water goes to enormous settling ponds, where the slime
settles down, gradually drains, and dries, and it is afterwards used
for various purposes during the smelting operations; being dug out in
the form of a fine clay. A new form of centrifugal apparatus (the Peck)
is now being installed for the separation of this material. The
subsequent treatment of the products from the concentrating operation
is indicated in the diagram (fig. 12), from which it will be seen that
the—
_Coarse Concentrates_, 1¼, ⅞ (and ⅜) inch size, are smelted
in the blast furnaces.
_Fine Concentrates_, 7, 5, 2½, 1½, and 1 millimetre size,
pass to the roasters, and thence to the reverberatory
furnaces.
_Slimes_ are used for briquetting, and several other operations.
_Tailings_ pass to the dump.
[Illustration: Fig. 12.—Outline of Smelting Scheme at the Anaconda
Smelter, Montana, U.S.A.]
_B._ =Agglomeration of Fines.=—It has just been seen that the wet
concentration of ores (considered advisable in a large number of
cases) results in the production of a considerable quantity of
fine concentrate, a form of material not well suited for immediate
blast-furnace treatment.
In addition, smelters often receive considerable amounts of fines in
the smelting-ore supply, which it is not unusual to screen out and to
treat separately from the coarser materials.[4]
The alternatives for the treatment of fines, and more particularly of
fine concentrate, include smelting in reverberatory furnaces (usually
after roasting); blowing into the converter (a new process still in
the experimental stage); and blast-furnace treatment after suitable
preparation.
Blast furnaces have many advantages which lead to their extended use in
copper smelting practice, but one important feature, which also applies
to the smelting of other metals, has always to be borne in mind in
this connection—viz., _that material in a finely divided state cannot
be treated directly in a blast furnace without heavy losses_, and the
working of the furnace on such charges is not efficient.
No material less than ¼ to ⅜ inch in size, especially when in the form
of sulphides, should be fed as such into a modern blast furnace. Fines
in the furnace lead to—
(_a_) _Accretions_,
(_b_) _Irregular working of the furnace and the charge_,
(_c_) _Clotting and low concentration_,
(_d_) _Heavy flue-dust losses_,
and their presence is often the cause of much trouble at many of
the modern smelters. The agglomerating of the fines is, therefore,
a very important preliminary in any scheme of treatment involving
the employment of the blast furnace on such material. Agglomerating
is usually performed by one of two methods—(1) briquetting, (2)
sintering. Of these, briquetting has hitherto been in very general
use, but several advantages connected with the sintering process and
the resulting product are leading to its adoption with much success in
several localities, and attracting for it considerable attention at
present.
(_a_) =Briquetting=.—Among the advantages of briquetting is the fact
that it utilises large quantities of the copper-bearing slime produced
at the concentrating plant, this material often possessing good binding
properties which render it very suitable for briquette-making.
[Illustration: Fig. 13.—Sketch Plan of Briquetting Plant.]
[Illustration: Fig. 14.—Section through Auger-Former, showing
Briquetting Mechanism, of Chambers’ Machine.]
[Illustration: Fig. 15.—Chambers’ Briquette-making Machine.]
The type of plant in use at different smelters varies considerably, the
method adopted being either the stamping out of the briquettes, or by
the application of steady pressure, the production of bars which are
then cut up to convenient size.
The constituents used depend naturally on the materials available at
the smelter, briquettes, both with lime and without, being made.
_The Briquetting Plant at Anaconda._—The operation of this plant
affords a good example of the process. Its working is very successful
in using up much fine concentrate, as well as the slime from the
ponds, which acts as binding material and at the same time supplies
copper. Briquette, indeed, constitutes one of the biggest items of
the charge for the Anaconda blast furnaces. There are four Chambers’
machines in use, making 840 tons of briquettes daily. The briquettes
consist of slime, fine first-class ore screenings (< ⅜-inch size),
fine concentrate from the dressing plant, and coke (which is recovered
from the reverberatory furnace gratings). The quantities used daily
are somewhat as follows, though they are naturally subject to some
variation, depending on supplies:—
Slime, 500 tons.
First-class ore screenings, 300 "
Fine concentrate, 200 "
Coke, 70 "
and the composition of the briquettes is about—
Copper, 5·0 per cent.
Ferrous Oxide, 16 "
Silica, 45 to 50 "
Sulphur, 15 "
Lime, 0·7 "
Moisture, 15·0 "
Coke, 5·0 "
The different materials are stored in bins, and fed through doors to
conveyors, which discharge on to an elevator leading to a divided
hopper, each division of which feeds a pug-mill. The pug mills are long
troughs in which inter-moving bladed spindles rotate, churning up the
materials; the mixing being assisted by a water supply from above. The
mixture passes down a chute to one end of an auger machine, from which
it issues, through a steel ring, in the form of a continuous slab,
6 inches × 4 inches in section, to a cutter 10 feet distant, which
slices off bricks 10 inches long, each of which weighs about 10 lbs.
The bricks pass to a traveller, thence by another to feed bins. The
briquettes are not dried, but are used just as made with 15 per cent.
of moisture, and are generally the last item of the charge to be added
on the car. They crumble slightly, but are sufficiently strong to stand
the handling during charging.
Many similar methods, including hand processes, are employed.
(_b_) =Sintering Processes.=—This method of treating fines involves
roasting reactions, as well as the mechanical process of agglomerating.
Whilst it thus furthers the concentration obtained in the subsequent
furnace operation, since it eliminates some sulphur, it also utilises
the fuel value of the fines, and yields a product which works well in
the blast furnace. Several processes have been introduced, and the
M‘Murty-Rogers method installed at Wallaroo, S. Australia, illustrates
very well the principles upon which this class of treatment depends.
It is a sintering and roasting process similar in type to the
Huntingdon-Heberlein method for lead smelting, but lime is not used
as a rule. It is employed primarily for fine concentrates which are
somewhat siliceous.
=Charge.=—Must contain 15 to 35 per cent. silica, and 15 to 25 per
cent. sulphur.
=Pots.=—8 feet 6 inches in diameter, when used for ore, and 4 feet 6
inches deep; with vertical sides. There is a false grate 10 inches
above the bottom, pierced with ⅝-inch holes.
=Blast.=—1,000 cubic feet per minute at 13 to 20 ozs. pressure per
square inch.
=Capacity=, 8 to 10 tons. =Time=, 8 to 10 hours.
=Method.=—Cover the grate with a layer of roasted material, light small
fire of wood, blow, and gradually charge in the ore whilst the blast
is on. Lime is unnecessary, but water is essential in the process, and
the ore must be very wet; 6 to 9 per cent. water being used for ore
charges, and 3 to 4 per cent. with rich mattes, otherwise working is
not uniform, and the losses by dusting are great. With the requisite
quantity of water present, the working is regular and uniform, there is
little dust, and the roasting is efficiently performed.
=Products.=—If ore is charged, a sintered mass of matte and ferrous
silicate results; if poor matte is used, the product is a rich matte
and ferrous silicate; and if rich matte is used, metallic copper and
ferrous silicate are obtained. At the end of the blow the charge is
tipped out and fed into the blast furnace.
=Costs.=—The method as employed at Wallaroo to treat 400 to 500 tons of
material per week, operated at a cost of 3s. 6d. per ton, or about 1s.
more per ton than for ordinary roasting.
Though this particular process is only, to the author’s knowledge,
employed at a few smelters, sintering or blast-roasting methods on
the same principle have been introduced at several other works, and
their adoption promises to lead to very successful results, being
particularly suited for the class of material indicated above. The
advantages claimed for the process are that—
(_a_) It saves heavy mechanical losses, such as those of
the dust resulting from calcining operations and from the
charging of hot calcines into reverberatory furnaces.
(_b_) It gives a product suitable for blast-furnace
smelting—often the cheapest and most convenient method of
working.
(_c_) It results in efficient roasting and good reduction
of sulphur, yields the product in an advantageous form for
subsequent smelting, and promotes a satisfactory removal of
impurities in the slag.
In addition, the process offers the possibility in the future of being
so modified as to leave in the adequately compacted products so much
sulphide that their fuel values can be realised in the blast furnace.
In other words, after the preliminary sintering process, to smelt the
(fine) sulphide-concentrates pyritically in the blast furnace.
Of the more recent types of machine for conducting the process of
sintering, that of Dwight and Lloyd is in operation at several
smelters. The moistened ore falls on to an endless chain conveyor,
composed of separate grids carried on wheels. The conveyor carries the
ore through the flame from a small furnace which starts its ignition,
and it is then drawn over a long suction chamber where air is sucked
through the hot mass, thus effectually roasting and sintering it. The
chamber has special devices which ensure the drawing in of the air
through the charge only, and so prevent inward leakage (see Fig. 16).
The sintered cakes are finally discharged automatically into cars.
Details regarding the machine vary at different smelters; at one works
the length is 30 feet, the rate of travel 8 inches per minute, and the
vacuum in the suction chamber 6 ozs.
The size of the particles should not exceed ¼ inch, and not more than
25 per cent. of the charge should be so large. Some 3 to 5 per cent.
tends to pass through the grids, and so be drawn into the suction
chamber; this is cleared out at intervals through special doors. Water
is necessary, and from 6 to 10 per cent. must be employed in uniformly
moistening the charge, which, by the addition of suitable fluxes,
is often made of such proportions that in subsequent blast-furnace
smelting a satisfactory slag is produced without further additions. The
sulphur reduction by the process is very considerable.
[Illustration: Fig. 16.—Dwight-Lloyd Sintering Machine.]
Such blast-roasting methods, with suitable modifications, promise to
assume considerable importance in the developments of modern smelting
practice.
_c._ =Roasting.=—Roasting is often a very important preliminary stage
in the scheme of treatment of copper ores. It was formerly considered
an essential operation in smelting processes for sulphide ores, the
material being crushed and concentrated largely with a view to such
subsequent treatment. This is not the practice in modern smelting.
Roasting is now only conducted where the necessity for it arises, as
in the case where wet dressing, having been considered advisable, has
resulted in the production of large amounts of fine concentrate, and
where reverberatory furnaces are installed for the smelting of this
material. Preliminary roasting of the concentrates then conduces to the
production of a matte of converter grade in one smelting operation.
=The Principles of Copper Smelting.=—Copper extraction from sulphide
ores is essentially an oxidation process, the iron and sulphur being
oxidised and the oxide of iron slagged away. All such smelting
processes, both the older and the more modern ones, are based on this
fact, and underlying all of them are certain fundamental principles
which it is essential to keep in mind in considering every phase of the
subject.
These may be summarised as follows:—
(1) In the melting down of a furnace charge, the copper has first claim
on any sulphur which may be present.
(2) Only such sulphur as remains in excess after the copper has been
satisfied, is free to combine with other constituents of the charge.
These fundamental principles can best be illustrated by following the
reactions during the smelting of a typical charge. Thus—
Copper—-+
\
+ ➡ Cu_{2}S—+
/ \
Sulphur—+ + ➡ × Cu_{2}S. yFeS ... _Matte_.
\ /
+ ➡ FeS—-—-+
/
Iron——-+
\
+ ➡ FeO——+
/ \
Oxygen—-+ + ➡ × FeO. ySiO_{2} ... _Slag_.
/
Silica ➡ SiO_{2}—+
The copper takes up sufficient sulphur to form Cu_{2}S; the remaining
sulphur combines with any iron which is available, forming FeS. These
two sulphides, dissolving in all proportions, constitute the _matte_
product of smelting.
The iron in excess of that required by the sulphur becomes oxidised,
and the resulting oxide combines with silica in the charge, forming the
silicate _slag_ of the smelting operation.[5]
It will thus be apparent that, in general, the larger the amount of
sulphur present in a furnace charge, the more FeS will there be in the
matte after melting, and the smaller will be the proportion of copper.
In consequence, the grade of the matte will be lower.
The proportion of sulphur in the charge thus controls the concentration
of the copper by the smelting operation, and, in order to effect the
desired concentration, oxygen is required in order to burn off sulphur
and to oxidise iron. There are two general methods of supplying this
necessary oxygen.
(1) By a preliminary oxidation of the charge outside the smelting
furnace—_Roasting_.
(2) By oxidation inside the smelting furnace itself—_The pyritic
principle_ (to be considered later).
=Modern Practice as regards Roasting.=—In modern copper smelting, the
tendency is to do away with roasting as much as possible.
_Objections to Roasting._—(1) Expense involved by a separate
preliminary process. This includes
(_a_) Preparation of the ore for roasting.
(_b_) Extra ground, and plant required for handling.
(_c_) Labour, fuel, etc., required.
(_d_) Extra handling of material before and after roasting.
(2) Heavy mechanical and other losses during the process.
(3) Loss of the fuel value of the iron and sulphur for smelting.
(4) Necessity, in the majority of cases, of having the ore in a
fine state of division in order to conduct efficient roasting, thus
militating against its subsequent use in the blast furnace, unless the
product receives preliminary agglomeration.
Thus at Tennessee, the cost of roasting was about 40 cents, or 1s. 8d.
per ton of ore (equivalent to ½d. on every pound of copper produced).
The cost for the year 1903 amounted to £19,000, employing 170 men
out of a total staff of 900 at mines and smelters. The conditions
for roasting were here exceptionally favourable. The closing of the
roast-yards set at liberty £34,000, which had been tied up in this
manner.
_Advantages of Roasting._—Illustrative of the conditions under which
roasting is advantageously conducted in modern practice, the case of
the Butte second-class ores may be quoted.
These ores contain about 5 per cent. of copper in the form of
sulphides, finely disseminated through large quantities of siliceous
gangue. Direct smelting in a blast furnace would not yield a matte
of the desired “converter” grade, except at very heavy expense
and difficulty. The ore is, therefore, wet-dressed up to 9 to 10
per cent. copper, and the coarse concentrates now help to yield a
good matte, when smelted in the blast furnace. By the wet-dressing
treatment, however, a considerable quantity of fine material is
unavoidably produced, for which the most convenient treatment in
such large quantities, under prevailing conditions, is in the
reverberatory furnace. The atmosphere of this type of furnace being
to a great extent neutral, the charge would tend simply to melt down
without very much reduction of sulphur, resulting in the production
of very low-grade matte. Roasting of these fine concentrates is,
therefore, desirable for reducing the sulphur to such an extent as
will yield a high-grade converter matte.[6] Roasting being thus often
advisable as a preliminary, its inclusion in a smelting scheme under
suitable conditions entails the following advantages over the direct
reverberatory treatment of unroasted ores:—
(1) It ensures satisfactory concentration on smelting.
(2) It leaves reverberatory furnace smelting practically
a remelting operation, and so affords exact control of
the concentration effected.
(3) The roaster gases may be utilised for making acid.
In modern practice the work of the reverberatory plant is controlled at
the roasters. The reverberatory foreman smelts whatever mixture is sent
from the roasting plant, and if the grade of the resulting matte is not
satisfactory, it is in the roasting operations that the required change
is made for the correct adjustment of the sulphur and for controlling
the consequent tenor of the matte.
=The Reactions of Roasting.=—The operation of roasting is the exposing
of a substance to the effects of heat and air, in order to oxidise it,
and to render it more suitable for subsequent smelting operations.[7]
In the case of the ordinary sulphide copper ores, roasting not
only (_a_) reduces sulphur, and so ensures good concentration on
smelting, but (_b_) by oxidising the iron, provides a ready flux for
siliceous gangues. The more important reactions occurring to the usual
constituents of the copper ores which are roasted, may be summarised as
follows:—
_Iron Pyrites._—First loses free sulphur at a low temperature: it is
generally assumed that FeS is left, but the residual sulphide rarely
attains this composition—
FeS_{2} ➡ FeS + S.
_Iron Sulphide._—Sulphur has a great affinity for oxygen, to form
SO_{2} and it may be assumed that this reaction first takes place thus—
FeS + O_{2} ➡ (Fe) + SO_{2} (i.)
The iron is however instantly oxidised by the excess oxygen always
present—
(Fe) + O ➡ FeO (?) (ii.)
Or, combining (i.) and (ii.)—
FeS + 3,O ➡ FeO + SO_{2}.
This sulphur oxidation is an important source of heat, and in the early
stages of roasting, sulphur is seen burning with the familiar blue
flame, and the mass becomes red hot; stirring being required to prevent
the material from sintering by the heat generated within itself.
The oxidation of the iron generally proceeds further, yielding higher
and more stable oxides—
┌─
│ 2FeO + O ➡ Fe_{2}O_{3}.
─┤
│ 3FeO + O ➡ Fe_{3}O_{4}.
└─
The SO_{2} in the presence of oxygen and in contact with strongly
heated material further tends to form SO_{3}, which is a powerful
oxidising agent, and plays a considerable part in the various oxidising
reactions which occur.
_Pyrrhottite_ behaves in much the same way; it may be regarded as
consisting of _x_FeS + a little extra sulphur. It does not roast quite
so easily as pyrites, partly on account of physical characteristics,
and partly because, in the case of pyrites, the greater amount of
excess sulphur which is first driven off, tends to leave the mass more
porous and so assists oxidation.
_Copper Sulphide._—Its characteristics on oxidation have already been
indicated in Lecture III., p. 36. It melts easily, often at roasting
temperatures, hence careful heating and attention are required when
much is present.
The reactions are probably analogous to those of FeS oxidation, in the
primary oxidation of the sulphur and the instantaneous oxidation of the
nascent copper—
┌─
│ Cu_{2}S + O_{2} ➡ (2Cu) + SO_{2}
─┤
│ (2Cu) + O ➡ Cu_{2}O,
└─
thus Cu_{2}S + 3.O ➡ Cu_{2}O + SO_{2};
this being accompanied by simultaneous action of the following nature:—
Cu_{2}O + SO_{2} + 2,O ➡ 2CuO + SO_{3}
CuO + SO_{3} ➡ CuSO_{4}
CuSO_{4} + Cu_{2}O ➡ 3CuO + SO_{2}.
In addition to the tendency to melt, copper sulphide roasts less
perfectly than the FeS, usually yielding oxides which are accompanied
by small quantities of sulphate.
_Chalcopyrite_ is the commonest copper ore, and the material most
frequently subjected to roasting in copper smelting practice.
Consisting of Cu_{2}S. Fe_{2}S_{3}, and accompanied usually by a
large excess of FeS_{2}, it behaves very much like a mixture of these
sulphides when treated in the roaster furnace, hence the reactions on
roasting follow on the lines just indicated.
In practice the roasting is never carried to such a degree that all the
sulphur is eliminated, since it is essential to retain some sulphur
in order to collect the copper in the form of matte, and also because
the time, and the cost of the fuel required to roast all of it off,
would be prohibitive. Consequently, the products from the roasting of
chalcopyrite consist principally of oxides of iron and copper, together
with a certain amount of copper sulphate, very little iron sulphate,
and some undecomposed sulphides.
The actual form in which the sulphur is present at the end of the
roasting operation is not usually of very special importance in
practice, especially where the previous experience with the roasted
material determines the extent to which the roasting is conducted,
since the greater part of the sulphur eventually produces the sulphide
and constitutes the matte, on smelting the roasted charge; although
some is also eliminated as SO_{2} by interaction with oxides. In
modern roasting practice, therefore, all that is usually required is
to roast the ore down to, say, 5 per cent., 6 per cent., 8 per cent.,
or whatever proportion of sulphur is necessary to yield the required
grade of converter-matte in the reverberatories, as judged by previous
experience of the furnace plant and working. Much SO_{2} is evolved
during the roasting, though it is usually largely diluted with nitrogen
from the air used up.
_Other Foreign Constituents of Copper Ores—Zinc Sulphide._—ZnS is
sometimes present. Some remains unchanged on roasting, as the heat in
ordinary practice is not great enough to thoroughly decompose it. Some
oxide and some sulphate are also produced.
2ZnS + 7,O ➡ ZnO + ZnSO_{4} + SO_{2}
is suggested by Peters as a probable reaction occurring to this
material under roasting conditions.
_Lead Sulphide_ is also occasionally present with copper ores. It melts
readily, and is not entirely decomposed at the temperatures employed
for the roasting of copper ores. The reactions on oxidation are largely
analogous to those for other sulphides.
┌─
│ PbS + O_{2} ➡ Pb + SO_{2}
─┤
│ Pb + O ➡ PbO
└─
or, PbS + 3.O ➡ PbO + SO_{2}.
Also, 2PbO + SO_{3} ➡ PbSO_{4}.PbO (basic sulphate).
_Arsenides_ are partly left as the corresponding oxides, whilst some
As_{4}O_{6} is evolved, and some basic arsenate generally remains.
Roasting Practice.
_Favourable Conditions for Successful Roasting._
(_a_) The sulphide should be in a finely divided form, so as to ensure
good contact with the air.
(_b_) The air should be supplied in a gentle current, so as to
continually provide fresh oxygen, and sweep away the inert gases which
are produced.
(_c_) The ore should be heated to a dull red heat, which is a condition
favourable for commencing the ignition and reactions. The temperature
should, of course, be well below a melting heat (_Peters_).
_The Apparatus for Roasting_ depends to some extent on the class of
material to be dealt with, which may be in the form of either (_a_)
lump ores, or (_b_) fine ores.
(=a=) =Roasting of Lump Ores.=—In modern copper-smelting work, the
practice of roasting lump ores is practically obsolete. The conditions
under which its use might still be justified are those associated with
newer mining districts, where rapid concentration of heavy sulphide
ore into matte is required, before the time is ripe for smelting the
material pyritically, and where further, it is desired to employ the
blast furnace for the smelting operations under these circumstances.
The advantages possessed by the method are—
(1) No preliminary crushing is required.
(2) The product is largely in the form of lumps, and hence
immediately suitable for blast-furnace work.
(3) The plant and appliances required are simple.
The two methods employed are—(A) open-air roasting, (B) roasting in
kilns.
A. _Open-air Roasting of Lump Ores._—This method is conducted in
heaps or stalls, and the features just considered apply particularly
to this branch of roasting practice. The modern tendency is to avoid
heap-roasting altogether, and it is only conducted when the conditions
are exceptional.
Amongst the many grave objections to open-air roasting are—
(_a_) It is very slow, since a long period of time is
required for the oxidising effect to penetrate through
massive lumps of ore.
(_b_) A large amount of capital is tied up in the material
at the roast-yards.
(_c_) The losses occasioned by wind and rain are very
considerable.
(_d_) It is difficult to use up a large quantity of fines in
the roast-heaps.
(_e_) Difficulties arise owing to damage by the fume, and
from interference by litigation.
There is one special instance of a modern smelter making a great
success of heap-roasting—namely, at Rio Tinto—but the circumstances are
peculiar, as the roasting is followed by leaching operations of the
immense ore heaps _in situ_.
This branch of roasting need not be considered at length, and the older
standard text-books give full descriptions of the various methods
employed. The following particulars are important, however, when under
exceptional circumstances such work has to be undertaken:—
The maximum and best average size under ordinary conditions is 40
feet by 24 feet, by 7 feet high above the bed of fuel. The height is
important, and varies with the quantity of sulphur in the ore. The
lower the sulphur content, the higher the pile; with about 40 per cent.
sulphur, the best height is 6 to 7 feet; with 15 per cent. of sulphur,
up to 9 feet; and if still less sulphur be present, the height may
even be a little greater. Such a heap holds about 240 tons, and if the
quantity of ore to be dealt with exceeds this, a number of such piles
should be constructed. The time occupied in roasting is about 70 days,
with 10 days more for removing and rebuilding.
The selection of a proper site is important.
(_a_) The prevailing direction of the wind must be considered,
so as to keep the fumes away from the works and offices.
(_b_) The yards must be protected from winds, so as to prevent
losses of dust, as well as uneven burning.
(_c_) The ground must be perfectly dry or drained.
Along the upper edges of the roast-yard a deep trench should be cut,
so as to catch rain-water, and prevent it from washing soluble copper
salts out of the pile; drainage trenches must also be provided to
carry any copper-bearing liquors to some point where the copper can
conveniently be precipitated on scrap iron. Enormous losses of copper
may occur if these precautions are not observed; thus, at one period in
the old roasting process in Tennessee, as much as 34 per cent. of the
copper in the heaps was lost in 186 days.
_Preparing of the Floor._—Remove roots and subsoil, fill space with
broken stone or rough tailings, cover with 4 to 6 inches of clayey
loam, and beat down well. The floor is then fairly impervious, and
does not crack on drying. The ground should be given a gentle slope so
as to facilitate draining. A layer (about 6 inches thick) of fine ore
is next put down, then 9 inches of fuel; channels are now mapped out
by means of logs set in both directions, leading to rough chimneys.
The pile is then constructed, with the lower parts of the very coarse
materials, smaller stuff being put towards the top and sides. On the
very top and at the outside of the pile are placed the fines, but this
top cover is only put on when the burning is well started. This process
is still worked at Tyee, B.C., and at some other localities, but is
most probably only a temporary plan, to be replaced by a more efficient
method as development progresses.
B. _Kilns for Lump Ores._—Kilns possess the advantage that they
permit of arrangements being made for the recovery of SO_{2} for acid
manufacture, and the subject belongs more properly to that branch of
technology. Few large smelting works employ kilns for roasting lump
ores, though there are important exceptions at works both in Britain
and on the Continent of Europe. Kilns are used at the Cape Copper
Company’s smelter at Britton Ferry, for this purpose.
(=b=) =The Roasting of Fines.=—Fines (and particularly fine
concentrates) are the usual materials subjected to roasting. The finer
the particles, the more rapid and complete is the oxidation, but the
losses by dust are heavier. The size limit is thus liable to some
variation, but often the material roasted is that under ⅜-inch in size.
_Roasting Furnaces—Requirements._—For the roasting of fines there is
simply required a place where the material can be gently heated in the
presence of a constantly renewed air supply. The fuel has itself a
reducing action, it must therefore be separated from the charge, and
hence the furnace employed is of the reverberatory type. Muffles are
never used for the oxidising roasting of copper ores. Since only a
moderate temperature is necessary for the operation, the furnace needs
but a small fireplace, and it is provided with a large hearth area. The
fuel used is one yielding the fairly long oxidising flame required.
_Developments of Roasting Practice._—The main objects sought in
roasting practice have been—
(1) To have as large a surface of material exposed to heat and
air as possible.
(_a_) By elongating and multiplying the beds of
the furnace.
(_b_) By furrowing and rabbling the charge.
(2) Continually to expose fresh surfaces of ore to oxidation.
(_a_) First by hand-rabbling.
(_b_) Later by movable furnace hearths.
(_c_) By mechanical rabbling.
(3) To obtain a continuous output—
(_a_) By mechanical charging, rabbling,
and discharging.
The Development of the Roasting Furnace.
A. FIXED HEARTH.—In Great Britain from 1583 onward, roasting in _small
reverberatory furnaces_ seems to have been the usual method, and up
to 1850 the furnaces appear to have been only of moderate dimensions,
with a single hearth, 16 feet × 13 feet 6 inches, constructed of
firebricks set on end, and with a fire-box 7 feet × 2 feet 3 inches × 18
inches. Rabbling was done by a long rake, the material being charged
and worked through one door. This method of working wasted time,
made the process intermittent, and caused continual cooling down of
the furnace, involving large fuel costs and much labour. The first
improvements were to lengthen the hearth, to add more working doors,
and to put the charge into the furnace by a hopper passing through the
roof. It was next found best to elongate the hearth still further, and
to drop the level of the bed in stages by about 2 inches at a time,
thus ensuring better control of working. By this means the best type of
_hand-calciner_ was arrived at, consisting of four beds, each 16 feet ×
16 feet, the whole charge being moved forward from one bed to the next
at each stage of the process.
In roasting, the ore is first placed in the coolest part of the
furnace, and is worked towards the fire, so that the charge travels
in one direction, and the flame and furnace gases in the opposite
direction to meet it.
The advantages of this system are that—
(_a_) The clotting of the sulphides is prevented, since
the first part of the roasting proceeds at a
comparatively very low temperature.
(_b_) The sulphur in the ore often provides sufficient
heat to maintain the roasting in progress during
the early stages.
(_c_) The hottest parts of the furnace are where the
roasted infusible oxides arrive, so but little
clotting or sintering occurs here.
The capacity of the four-bedded hand-roaster is 7 to 15 tons per
twenty-four hours, depending on the sulphur proportion in the charge
and in the roasted product.
It is a very useful form of furnace when labour is cheap. The furnace
works very efficiently, but in the New World, where manual labour was
dear, labour costs became prohibitive, and in order to economise in
this direction, mechanical rabbling was introduced.
_The O’Harra Calciner_ (1885) was essentially the old type of furnace,
double hearthed and mechanically rabbled. It consisted of long straight
furnace hearths. The rabbles were ploughs dragged through the furnace
by means of endless chains which were carried over grooved pulleys,
situated outside the furnace, at the ends. This was an important
invention, giving a continuous feed and discharge, a much larger
output, and efficient and regular stirring without much hand labour.
The rabbles became cooled on issuing from the hearth. The capacity was
50 tons per day from furnaces of 90 feet × 9 feet hearths, giving a
roasting capacity of 61 lbs. of ore per square foot of hearth area,
compared with about 33 lbs. per square foot with the old hand calciner.
In working the early forms of this furnace there were many mechanical
troubles and breakdowns, and the subsequent modifications of this
form consisted largely of devices for the purpose of overcoming such
difficulties.
_Modifications and Improvements._—_Allen_, instead of a rope to carry
the ploughs, used small wheeled carriages, running on a track which was
laid along the floor.
_Brown_ (important) ran the carriages along narrow corridors at either
side of the hearth, so as to protect the ropes and carriages from the
very corrosive action of the furnace gases. A continuous narrow slit
along the inner wall of the corridors allowed the arm carrying the
plough to travel forward.
_Wethey_; _Keller_; worked on very similar principles. The chief
improvements were in details, and had for their object the prevention
of wear and tear, and of the break-down of parts.
_Prosser._—Very similar; used at Swansea Works.
_Ropp._—The carriage runs underneath the bed, and supports a vertical
shaft which passes through a slot along the furnace hearth and carries
the arms furnished with ploughs.
[Illustration: Fig. 17.—O’Harra Furnace (Fraser-Chalmers), illustrating
Principle of Mechanical Rabbling by Travelling Ploughs.]
The Ropp and Prosser calciners work very successfully. The hearth is
about 105 feet long × 11 feet wide, with a capacity of about 36 tons
per day.
[Illustration: Fig. 18.—Section through Mechanically Rabbled Roaster
Furnace (illustrating Improvements for Protecting Driving Mechanism).]
_Brown Horse-Shoe Furnace_ operates on the same principle as the above,
except that the hearth is bent round in order to save space.
_Pearse-Turrett_ (1892 at Argo).—In this type of furnace the bed is
curved round in the form of a circle. The rabbling ploughs are carried
at the ends of arms which are attached to an upright rotating spindle.
The spindle is set in the centre of the space enclosed by the circular
hearth.
In all the above classes of furnace, the firing is done, when
necessary, from fireplaces built at intervals along the sides of the
furnace; either coal or gas being employed as fuel.
B. ROTATING HEARTHS.—This type of furnace is still reverberatory, but
instead of making use of mechanical rabbling, the hearth rotates, in
order to give agitation to the materials and assist their discharge.
(_a_) _Intermittent Working—The Brückner Roaster._—The details and
working of this roaster are familiar. The furnace was invented in 1864
for gold and silver ore-roasting in Colorado, and was later introduced
for the roasting of copper ores, being at one time the furnace most
commonly used for the purpose. It was employed all over the Western
States, and at one works alone, 56 were at one time in use.
The usual length was 18 feet 6 inches and the diameter, 8 feet 6
inches; giving an output of about 12 tons per twenty-four hours. It was
furnished with a removable fireplace, used to start the roasting. The
operation could then be allowed to proceed by itself, the fireplace
being wheeled away to another hearth, and being eventually brought
back to the first hearth for about three hours, in order to give the
required higher finishing temperature. Several dust chambers were
attached to this, as to all forms of roasting furnaces, which by their
nature and manner of work are apt to produce considerable quantities of
dust.
The advantages of the Brückner cylinder lay largely in the fact that
it afforded good control of the sulphur contents in the charge,
since the ore could be retained in the furnace until the sulphur was
sufficiently low. The furnace is simple to work, and not so liable to
get out of order as many other forms. It possesses however, distinct
disadvantages in that its working is intermittent, its use involves
comparatively high fuel costs, whilst the discharging presents
considerable difficulty and trouble to the labour employed, on account
of the awkwardness and the high temperature of the discharge, and the
sulphurous gases evolved.
Its use has now been very largely discontinued.
_Improvements_—(_b_) _Continuous Working._—The continuous type of
roasting furnace of this class involves the use of sloping cylindrical
hearths which rotate, and so agitate and help to discharge the
materials.
_Oxland_ (1868) first introduced this type in Cornwall, for the
roasting of tin ores.
The Oxland furnace was an inclined cylinder, the material was fed in
at the top, and by the rotation of the cylinder the charge gradually
travelled downwards, approaching nearer and nearer to the fire, and
being discharged close to the fire-box.
_White_ (1872) improved this furnace, and the White cylinder is largely
used in South Wales. The cylinder revolves slowly by friction gearing;
inside are four lines of projecting brick-work which form a shelf, thus
assisting the agitation of the charge.
_The White-Howell Furnace_ is somewhat similar to the White, but is
unlined for the greater part of its length, except at the lower end
near the fire-box, where it is much wider and is bricked. It is stated
to work more satisfactorily than the older form, having a larger
capacity and using but little fuel.
The furnace is employed at the Cape Copper Works, South Wales, for
matte-roasting. It is here 60 feet long, 7 feet diameter, inclined 6
inches in 60 feet, makes 8 revolutions per hour, and has a capacity of
10 tons of charge per day.
_Argall Furnace._—Consists essentially of four narrow tubes bound
together, each 28 feet long, 2 feet diameter, and lined. It works
rapidly, having a capacity of 40 to 50 tons per day, but is used more
for the roasting of cupriferous gold ores than at the copper smelters.
C. THE MACDOUGAL TYPE.—The most important form of modern roaster
furnace, and that most generally employed, is the MacDougal type. The
first furnace on this principle was invented by Parkes in 1860. The
design embodied two hearths, one above the other. Vertically down the
centre of these passed a spindle, supporting arms from which were
suspended the ploughs, and the rotation of this spindle carried the
arms over the beds.
As devised by Parkes, various mechanical difficulties were found,
and the working was intermittent, but the principle was recognised
as important. MacDougal in 1873 introduced his modification of the
furnace, primarily for the roasting of pyrites, at a Liverpool works,
and this form has now supplanted many of the older types for copper ore
roasting, and is in operation at most of the new smelting works.
_Principles of the MacDougal Type._—The furnace consists of an iron
cylinder lined with brick. Six circular hearths are constructed inside,
one above the other, and the vertical spindle carrying the arms and
ploughs for each hearth passes through the centre of the furnace. The
ore is ploughed towards openings on each hearth, which communicate
with the hearth below; the charge thus travelling from the outer edge
towards the centre, through the central opening to the middle of the
next floor, then outwards to the openings at the edge, and so on. The
original MacDougal furnace was 12 feet high and 6 feet in diameter. It
was improved by Herreshof in the direction of better rabbling mechanism
and greater ease of repair. The central spindle was an air-cooled
shaft, the supporting arms were made so as to be easily removable
from the shaft to facilitate repairs, and the furnace was enlarged.
Herreshof used air-cooling for the spindle and arms, as shown in Fig.
20.
[Illustration: Fig. 19.—MacDougal Roaster—Vertical Section.]
[Illustration: Fig. 20.—Herreshof Furnace—Section indicating
Connections for cooling Rabbles and Spindles.]
Evans, and subsequently Klepetko, in working the furnaces in Montana,
introduced, in about 1892, various marked improvements. The dimensions
were increased, enlarging the output. The spindle and arms were
water-cooled, which improvement removed much of the great difficulty
in working the MacDougal furnace, where the rapid wearing out of
working parts, and the difficulty of their removal, repair, and renewal
interfered greatly with efficient working.
Many of these troubles have now been overcome in the Evans-Klepetko
type, and in the still further improvements since made at Anaconda.
The general arrangement of the floors, spindles, arms and other
details shown in the Herreshof furnace (Fig. 20) are preserved in the
Evans-Klepetko and similar types of roaster; the chief alterations are
in matters of detail, the results of which have however, been important.
Furnaces of this improved kind are now used all over the West; there
are 64 at Anaconda, Mont.; 32 at the International Smelter, Tooele,
Utah; 24 at Garfield, Utah; 16 at Steptoe, Nevada; and also at
Balakala, Cal., Cerro de Pasco, Peru, and other large smelting centres.
_Important Advantages._—Of the marked advantages of this type of
furnace, the following are perhaps the most striking and important:—
(1) There is a great saving of floor space by having the six
hearths one above the other.
(2) The use of a central common spindle carrying the arms
and ploughs simplifies the mechanism.
(3) The form is convenient for the compact arrangement of
a roasting plant of many units for feeding, discharge,
and supervision.
(4) Very little heat is lost by radiation, as the heat
passes mostly from one hearth to another.
(5) Very little fuel is required, none with heavy sulphides
(except for starting), as the heat of oxidation of the iron
and sulphur usually yields a high enough temperature to keep
the operation going. The fuel costs are lower than in other
types of roaster.
(6) Thorough rabbling, greater uniformity and better mixing
of product, continuous and regular feed and discharge are
obtained.
(7) The roasting is thorough, and perfect control of the
degree of oxidation is ensured by adjusting the rate of
passage of the ore through the furnace, which is regulated
by varying the ore feed and the speed of rotation of the
rabbles.
(8) Great saving in labour costs and difficulties. The
labour in roasting plants is extremely arduous, on account
of the high temperature of the material, and is dangerous on
account of the atmosphere.
=The Evans-Klepetko-MacDougal Roasting Furnace Plant at Anaconda.=—The
roasting plant at Anaconda formerly consisted of 56 Brückner cylinders,
which were eventually all scrapped and replaced by new plant of the
MacDougal type, subsequently greatly modified and improved as one
difficulty after another had to be overcome.
The saving in working costs resulting from this replacement of the
Brückners by MacDougal roasters is reckoned at about 5 cents (2½d.) on
every ton of calcines treated.
The roasters are arranged in four rows of 16 each, running east and
west. The charge cars travel along tracks at a height of 20 feet above,
discharging into rows of bins, one situated over each calciner.
[Illustration: Fig. 21.—Spindle Connections and Guide Shields of
Evans-Klepetko Roasters.]
_Details of Furnace._—Height, 18 feet 3½ inches; diameter, 16 feet. Six
hearths. The spindle is made in three lengths, each to carry the arms
for two hearths; it is 18 inches in diameter and is water-cooled. The
rabble arms are 6 feet long, half round, and flanged on the lower side;
they too, are hollow and water-cooled. The rabble-blades were formerly
cast in one piece with base plate, so as to slide on to the arms, but
are made now with detachable blades, which slide into grooves on the
base plate, so as to facilitate removal for repairs; the blades are 6
inches square and 1½ inches thick (Fig. 32).
The arms on separate floors are set alternately at right angles. Of the
two arms for each floor, one carries six blades, the other seven, so
that the furrows resulting from one set of blades are turned over by
the other. The blades are set so as to direct the ore from the outer to
the inner edge or _vice versâ_, according to the particular hearth. The
spindle and connections are protected from falling ore by shields which
are bolted on. The rabbles move slowly, making a 2½-inch furrow in a
5-inch layer of material.
_Capacity._—40 to 45 tons per day each, reducing the sulphur in the
charge from 30 per cent. to about 8·0 per cent. The output of the plant
is about 3,000 tons of calcines daily.
_System of Working._—Since reverberatory furnaces are used essentially
as remelting furnaces only, the roasting plant is operated so as to
yield a product of such composition as will directly produce a suitable
matte and slag on melting in the reverberatories. The fluxes required
for the calculated reverberatory charge are, therefore, sent through
the roasters mixed with the fine concentrate; such practice possessing
many advantages. The charge thus consists of fine concentrate from the
concentrator settling tanks, and screened lime-rock flux (too fine to
be used in the blast furnaces). The limestone lightens the charge,
decreases the tendency to clotting of the pure sulphides, chemically
assists oxidation, preheats and thoroughly mixes the flux, and ensures
a uniformly mixed charge for the reverberatory furnaces; whilst the
extra cost involved is but very small.
Three per cent. of lime is used; 40 tons of concentrates, 1¼ tons of
lime-rock, and 1¼ tons of flue-dust being charged per twenty-four hours
per furnace, through an automatic gravity feed, the opening of which is
closed and opened by an eccentric. The speed of the eccentric and the
extent of the opening are adjustable.
_Working._—Charge contains 25 to 35 per cent. sulphur.
[Illustration: Fig. 22.—Rabble-blades and Bases.]
_1st Hearth._—Temperature about 230° C. (black heat). This is
practically a drying floor, and the wet ore wears the rabbles away
rather quickly. Special forms of plough are being introduced. About 4
per cent. of sulphur is driven off from the pyrites.
_2nd Hearth._—Hotter; not quite red, except near outer edge. About 5
per cent. of sulphur burnt off.
_3rd Hearth._—Bright red heat (about 700° C.). Sulphur can be seen
burning off the ridges of calcines, with a blue flame. 5 per cent. of
sulphur eliminated. There is some clotting, and the sinter sticks to
the rabble-blades, and has to be barred off occasionally.
_4th Hearth._—Bright red heat (about 750° C.), uniformly bright, but
the flame has ceased. Sulphur loss, 4 per cent.
_5th Hearth._—The hottest (800° C.). Bright red.
_Bottom Hearth._—Cooler, dark red (about 650° C.). The doors on this
floor are left open. The charge is guided towards openings at the outer
edge to discharge chutes whilst still red hot, and it is fed from here
whilst hot into the reverberatory furnace-bins.
Efficient dust catchers and settlers are essential on the roasting
plant. The gases escaping at a temperature of about 315° C. contain 2
per cent. of SO_{2} by volume, 5 per cent. by weight. The ore takes
2¼ hours to pass through the furnace. Practically no fuel is required
except to warm up the roaster on commencing work.
_Labour._—The requirements are small. There is one general foreman
for the plant, and two helpers for each set of four furnaces. The
conditions are rather trying, especially during the discharge of the
calcines into the reverberatory charge cars.
ROASTING ORES POORER IN SULPHUR, IN MACDOUGAL ROASTERS.—The Anaconda
concentrates carry sufficient sulphur (33 per cent.) to supply all
the heat necessary for carrying out the roasting operations. When the
sulphur is below this requisite quantity, some extra heating may be
required, though, on the other hand, the reduction which is necessary
in the sulphur contents is lessened, depending, of course, on the
proportions of copper and iron in the charge. At Garfield, Utah,
where the concentrate only contains 20 per cent. of sulphur, the fuel
required for all roaster purposes is equivalent to 0·2 per cent. of the
charge, one of the calcines’ outlets being converted into a fireplace.
Here the output per furnace per day approaches 55 tons, roasting the
sulphur from 20 per cent. down to 10 to 11 per cent. The flue-dust
losses at this plant are 6 per cent., so efficient dust catching
appliances are essential.
=The Costs of Roasting in the MacDougal Furnace.=—Ricketts has recently
published a valuable analysis of the costs of the roasting operations
at the Cananea Smelter. The figures must, however, be understood to
apply strictly to the conditions prevailing at this particular camp.
The roaster plant consists of 32 improved MacDougal furnaces. The
charge supplied to the roasters assays—
Copper, 5·2 per cent.
Iron, 28·4 "
Sulphur, 29·9 "
Silica, 23·6 "
Alumina, 3·7 "
whilst the product (“calcines”) has an average composition of
Copper, 6·3 per cent.
Iron, 34·5 "
Sulphur, 7·7 "
Silica, 28·6 "
Alumina, 4·4 "
The plant operated on the following quantities of material, from
February to July, 1911, inclusive:—
Concentrates, 32,929 short tons = 76·08 per cent. of charge.
Fine sulphide ores, 9,590 " = 22·16 " "
Limestone, 762 " = 1·76 " "
—————— ——————
Total charge, 43,281 " = 100·00 " "
Weight of “calcines”
produced, 35,533 " = 82·10 " "
—————— ——————
Shrinkage, 7,748 " = 17·90 " "
====== ======
The total costs of roasting (from roaster charge-bins to reverberatory
furnace) worked out at 38·45 cents per ton, the distribution of these
costs being as follows:—
Total Costs. Cost per Dry Ton.
Sampling, $222·62 $0·0051
Bedding, 2,016·27 0·0466
Reclaiming, 3,072·71 0·0710
Operating furnaces, 7,680·58 0·1775
Hauling calcines, 911·01 0·0210
General expenses, 1,639·99 0·0379
———————— ——————-
Total direct costs, $15,543·38 $0·3591
Cost of flux, 1,097·85 0·0254
———————— ——————-
Total costs, $16,641·23 $0·3845
========== =======
ANALYSIS OF COST—
(1) _Operating_—
Labour, $7,398·56 $0·1709
Power, 1,577·64 0·0365
Fuel, 773·08 0·0179
Water, 78·71 0·0018
Sundries, 10·30 0·0002
Flux, 1,097·85 0·0254
—————————— ——————-——
$10,936·14 $0·2527
(2) _Repairs_—
Labour, $2,507·35 $0·0579
Shop expense, 361·00 0·0083
Supplies, 2,836·74 0·0656
———————-—— ————-——
Total costs, $16,641·23 $0·3845
========== =======
References.
Peters, E. D., “Principles” and “Practice of Modern Copper Smelting.”
Cloud, T. C., “The M‘Murty-Rogers Process for Desulphurising Copper
Ores.” _Trans. Inst. Min. and Met._, vol. xvi., 1906–7, p. 311.
Hofman, H. O., “Recent Progress in Blast Roasting.”
_Bulletin Amer. Inst. Min. Eng._, No. 42, June, 1910.
Austin, L. S., “The Washoe Plant of the Anaconda Copper Mining
Company.” _Trans. Amer. Inst. Min. Eng._, vol. xxxviii.,
1906, p. 560.
Rickets, L. D., “Developments in Cananea Practice.”
_Engineering and Mining Journal_, Oct. 7th, 1911, p. 693.
Redick F. Moore, “Recent Reverberatory Smelting Practice.”
_Engineering and Mining Journal_, May 14th, 1910, p. 1021.
See also—
Pulsifer, H. B., “Important Factors in Blast Roasting.”
_Met. and Chem. Eng._, 1912, vol. x., No. 3, March,
pp. 153–159. (With good Bibliography.)
Editorial Correspondence, “Sinter-Roasting with Dwight-Lloyd
Machines at Salida, Col.” _Ibid._, 1912, vol. x., No. 2,
Feb., p. 87.
Dwight, A. S., “Efficiency in Ore-Roasting.” _School of
Mines Quarterly_, 1911, vol. xxxiii., No. 1, Nov., pp. 1–17.
LECTURE V.
REVERBERATORY SMELTING PRACTICE.
Functions of the Reverberatory Furnace — Requirements
for Successful Working — Principles of Modern
Reverberatory Practice — Operation of Modern Large
Furnaces — Fuels for Reverberatory Work; Oil Fuel;
Analysis of Costs — Condition of the Charge.
=The Functions of the Reverberatory Furnace.=—The reverberatory
is essentially the furnace for the smelting of fine material, as
the comparatively still atmosphere, the absence of blast, and the
opportunities for settling prevent the heavy losses by dust which
necessarily accrue with the other types of smelting furnace. The
atmosphere of the furnace is practically neutral, it therefore
exercises little influence on the reactions taking place in the charge,
and the reverberatory is, in consequence, mainly a melting furnace.
Its functions are:—
(_a_) To allow of the formation, from the mixture of sulphides
and oxides in the roasted materials from the calciners,
of a copper matte and a slag.
(_b_) To maintain such a high temperature as to render these
products perfectly fluid, and thus to allow the matte and
slag to settle and separate thoroughly.
In spite of the neutral atmosphere, however, the smelting of the
roasted materials usually results in a higher concentration than would
be expected from the calculation of the sulphur, copper, and iron in
the charge. The reason of this is that the smelting operation results
in some further elimination of the sulphur, which causes the production
of a higher grade matte. This additional elimination of sulphur in the
reverberatory furnace smelting of the roasted charge is due to the
reactions which take place on melting, between the oxides, sulphates,
and sulphides of copper, all of which exist in the products from the
roasters. These reactions are expressed by the equations—
Cu_{2}S + 2Cu_{2}O ➡ 6Cu + SO_{2}
Cu_{2}S + CuSO_{4} ➡ 3Cu + 2SO_{2},
which indicate a further addition of copper to the matte, and a
corresponding loss of sulphur. Thus a typical reverberatory charge of
the following composition:—
Silica, 27·2 per cent.
Iron, 31·0 "
Lime, 2·3 "
Sulphur, 8·4 "
Copper, 8·3 "
should theoretically yield, on melting down, a matte running—
─┐ ┌─ ─┐ ┌─
[8]Cu (8·3) -> Cu_{2}S 10·4 │ │ Cu 8·3 │ │ Cu 30 %
├─ = ─┤ S 8·4 ├─ or ─┤ S 30 %
S (8·4−2·1) -> FeS 17·6 │ │ Fe 11·3 │ │ Fe 40 %
─┘ └─ ─┘ └─
In actual practice however, the matte resulting from the reverberatory
smelting of the charge had the composition—
┌─
│ Cu 45 per cent.
─┤ S 27 "
│ Fe 28 "
└─
the 3 per cent. loss of sulphur causing a …