The Project Gutenberg eBook of Pigments, Paint and Painting: A practical book for practical men This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Pigments, Paint and Painting: A practical book for practical men Author: George Terry Release date: January 9, 2018 [eBook #56344] Language: English Other information and formats: www.gutenberg.org/ebooks/56344 Credits: Produced by Chris Curnow, Chuck Greif and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) *** START OF THE PROJECT GUTENBERG EBOOK PIGMENTS, PAINT AND PAINTING: A PRACTICAL BOOK FOR PRACTICAL MEN *** Produced by Chris Curnow, Chuck Greif and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) PIGMENTS, PAINT AND PAINTING PIGMENTS, PAINT AND PAINTING _A PRA

source: Project Gutenberglicence: Public domain (per item)database: /home/dbs/gutenberg.dbmode: tablerecords: 544887 (max_rowid)citation: https://www.gutenberg.org/

The Project Gutenberg eBook of Pigments, Paint and Painting: A practical book for practical men

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: Pigments, Paint and Painting: A practical book for practical men

Author: George Terry

Release date: January 9, 2018 [eBook #56344]

Language: English

Other information and formats: www.gutenberg.org/ebooks/56344

Credits: Produced by Chris Curnow, Chuck Greif and the Online
Distributed Proofreading Team at http://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)

*** START OF THE PROJECT GUTENBERG EBOOK PIGMENTS, PAINT AND PAINTING: A PRACTICAL BOOK FOR PRACTICAL MEN ***

Produced by Chris Curnow, Chuck Greif and the Online
Distributed Proofreading Team at http://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)

PIGMENTS, PAINT

AND

PAINTING

PIGMENTS, PAINT

AND

PAINTING

_A PRACTICAL BOOK FOR PRACTICAL MEN_

BY

GEORGE TERRY

[Illustration: colophon]

London
E. & F. N. SPON, 125 STRAND
New York
SPON & CHAMBERLAIN, 12 CORTLANDT STREET
1893

INTRODUCTION.

In days gone by, the painter who served the usual term of
apprenticeship was deemed to have done all that was required to
qualify him for his trade. He may have learned little or much, but he
had “served his time,” and that was all that was expected of him. So
far as it went, the training was good, because it was nothing if not
practical, and practice is an essential element of skill. But nowadays
such a training can only be considered partial; mere practice, without
any scientific knowledge of the principles which underlie it, is but
half a qualification for the workman who aims at being really a master
of his trade.

When competition was unknown, and the low prices of raw material
offered no inducement for passing off inferior or fraudulent
substitutes, there was less need for a high degree of knowledge.
But under modern conditions, the painter who is unable to gauge the
qualities of the materials he uses, and who is ignorant of the rules
which govern those qualities, and of the principles which determine the
use of this and the rejection of that article, cannot long survive in
the struggle for supremacy or even livelihood.

Hence the need for a handbook such as this volume aims at being.
Granted that our technical schools and colleges are affording a liberal
and invaluable education to the workman who will avail himself of
the opportunities given him, still a man does not remain for ever at
school, and he needs a guide-book, handy of reference and accessible in
price, to refresh his memory and supplement the information gained in
the class-room and workshop.

To fulfil this useful purpose is the aim and object of this
unpretending volume.

CONTENTS.

CHAPTER I.

PRELIMINARY.

PAGE

Colour 1

Pigments 3

CHAPTER II.

BLACKS.

General 5

Animal-black 6

Bone-black 6

Frankfort or Drop-black 11

Ivory-black 11

Lamp-black 11

Unimportant blacks--Aniline,
candle, charcoal, coal, cork,
German, iron, lead, manganese,
Prussian, prussiate,
Spanish, tannin 25

CHAPTER III.

BLUES.

Cobalt blues--Cœruleum;
Cobalt blue; smalts 27

Copper blues--Bremen
blue; Cæruleum; Lime
blue; Mountain blue or
Azurite; Péligot blue; Verditer 34

Indigo 42

Manganese blue 49

Prussian blue--General;
Yellow prussiate; Combination
of the cyanide and iron
solutions; Antwerp blue;
Bong’s blue; Brunswick
blue; Chinese blue; Paris
blue; Saxon blue; Soluble
blue; Turnbull’s blue 49

Ultramarine 70

CHAPTER IV.

BROWNS.

Asphalt or Bitumen 101

Bistre 101

Bone brown 102

Cappagh brown 102

Cassel earth 102

Chicory brown 102

Cologne earth 102

Manganese brown 103

Mars brown 103

Prussian brown 103

Rubens brown 104

Sepia 104

Ulmin 105

Umbers 105

Vandyke brown 107

CHAPTER V.

GREENS.

Baryta 109

Bremen 112

Brighton 112

Brunswick 113

Chinese 118

Chrome 118

Cobalt 119

Douglas 120

Emerald 121

Guignet’s 125

Lokao 129

Malachite 129

Manganese 130

Mineral 130

Mitis 130

Mountain 131

Paris 132

Prussian 132

Rinmann 132

Sap 132

Scheele’s 133

Schweinfurth 134

Terre verte 134

Titanium 135

Verdigris 135

Verditer 136

Verona earth 136

Victoria 137

Vienna 137

Zinc 137

CHAPTER VI.

REDS.

Antimony vermilion 138

Baryta red 143

Cassius purple 143

Chinese red 144

Chrome orange 144

Chrome red 144

Cobalt pink 144

Cobalt red 144

Colcothar 145

Derby red 145

Indian red 147

Lead orange 147

Minium 148

Orange mineral 150

Oxide reds 150

Persian red 153

Realgar 153

Red lead 153

Rouge 153

Venetian red 153

Vermilion 153

Victoria red 169

CHAPTER VII.

WHITES.

Baryta white 170

Blanc fixe 172

Charlton white 172

China clay 172

Enamelled white 183

English white 183

Gypsum 183

Kaolin 183

Lead whites or White leads 183

Lime white 245

Lithophone 245

Magnesite 245

Mineral white 245

Orr’s enamel white 245

Paris white 246

Permanent white 246

Satin white 246

Spanish white 246

Strontia white 246

Terra alba 246

Whiting 246

Zinc whites 247

CHAPTER VIII.

YELLOWS.

Arsenic yellow 257

Aureolin yellow 257

Cadmium yellow 258

Chrome yellows 258

Gamboge 270

King’s yellow 271

Naples yellows 271

Ochres 272

Orpiment 280

Realgar 280

Siennas 281

CHAPTER IX.

LAKES.

Brazil-wood lake 283

Carminated lake 283

Carmine 283

Cochineal lake 284

Madder lake 284

Yellow lakes 285

CHAPTER X.

LUMINOUS PAINTS 286

CHAPTER XI.

EXAMINATION OF PIGMENTS.

Fineness 293

Body or covering power 293

Colour 293

Durability 294

CHAPTER XII.

VEHICLES AND DRYERS.

Generalities 295

Ground-nut oil 297

Hempseed oil 298

Kukui or Candle-nut oil 298

Linseed oil 299

Menhaden oil 303

Poppy-seed oils 305

Tobacco-seed oil 306

Walnut oil 307

Wood or Tung oil 308

Extraction of seed oils 308

Dryers 316

Litharge 316

Cobalt and manganese benzoates 318

Cobalt and manganese borates 318

Resinates 318

Zumatic dryers 318

Manganese oxide 318

Guynemer’s dryer 319

Manganese oxalate 319

Boiled oil 320

CHAPTER XIII.

PAINT MACHINERY.

Wright & Co’s 339

Hind and Lund’s 345

Brinjes & Goodwin’s 346

CHAPTER XIV.

PAINTING.

The surface 351

Priming 352

Drying 353

Filling 354

Coats 355

Brushes 355

Water-colours 356

Removing odour 356

Discoloration 356

Composition 358

Area covered 360

Measuring 360

Carriage and Car painting 361

Woodwork painting 368

Iron painting 369

Fresco painting 378

INDEX 383

ILLUSTRATIONS.

FIGURE PAGE

1, 2. BONE-BLACK FURNACE 8

3-11. APPARATUS FOR MAKING LAMP-BLACK 12-22

12. FURNACE FOR ROASTING COBALT ORES 31

13. FURNACE FOR MAKING SMALTS 33

14-17. YELLOW PRUSSIATE FURNACE 60

18-20. HANNAY’S WHITE LEAD FURNACE 217

21-25. LEWIS’S WHITE LEAD FURNACE 226, 230

26, 27. MACIVOR’S WHITE LEAD PROCESS 233, 239

28. APPARATUS FOR MAKING ZINC OXIDE 248

29. APPARATUS FOR MAKING ZINC SULPHIDE 253

30-32. FURNACE FOR ROASTING OCHRES 278

33-39. APPARATUS FOR EXTRACTING SEED-OILS 309-315

40-44. WRIGHT & CO.’S PAINT MILLS 340-344

45. HIND & LUND’S PAINT MILL 346

46-48. BRINJES AND GOODWIN’S PAINT MILLS 347, 348

49. NOAKES & CO.’S METALLIC KEG 350

CHAPTER I.

PRELIMINARY.

=Colour.=--The term “colour” is inappropriately given by common usage
to material substances which convey a sense of colour to the human eye,
but is properly restricted to that sense itself. The material colour
should be called “pigment” or “dyestuff” in the raw state, and paint
when compounded with other substances for application in the form of a
coating.

The sense of colour is due to light. In the absence of light there
is no colour, only blackness; and black is really no colour, but an
absence of colour. Very many conditions combine to cause different
colour sensations, some of which are understood, while others we are
not able to explain.

For instance, take the action of heat upon a solution of chloride of
cobalt. As soon as the liquid becomes warm, the pink colour disappears
and gives place to blue; but on pouring water into it, the blue
vanishes and the pink reappears. Again, on heating the blue crystals
of sulphate of copper they become white, but the blue colour comes
back when water is added, and the solution assumes a deeper tint as it
dissolves more of the white powder.

If all the rays are cut off from an electric light except those which
are in and beyond the violet, and a flask containing a solution
of sulphate of quinine is held in that portion of the spectrum, it
will become luminous. The same thing will occur even more strikingly
on placing a piece of uranium glass in the ultra-violet rays. The
explanation of this phenomenon is that beyond those rays which give
light there are others which do not give light, i. e. which do not
cause us to experience the sensation of light; the reason being that
their vibrations are too rapid. But when certain other substances, such
as sulphate of quinine, or a thin slip of uranium glass, are placed in
the path of the rays, this rapid motion is arrested and modified, and
these rays, which in themselves are not luminous, are reflected back
to our eyes as luminous rays. The rapidity of the vibrations being
moderated, our retinas become sensible to them as rays of blue light.

Colour does not depend only upon chemical composition nor solely upon
the aggregation of the particles, but upon these and other things
besides not yet explained. All matter is in a state of motion. If
you heat a substance you communicate an increased activity of motion
to the particles of which it consists. When certain coloured rays of
light are falling upon a substance, these coloured rays of light have
a motion peculiar to themselves. It may be that the degree of motion
in that substance, either existing in it naturally without heating,
or communicated to it by artificial heating, is such that these rays
of light are precisely those which that substance is not capable of
sending back to our eyes. They are then absorbed or destroyed in some
way, by the particular state of that substance upon which they fall;
and those rays which the substance is capable of reflecting back are
mainly sent back to our eyes. Certain colours, such as blue, yellow,
and green, absorb certain rays more or less perfectly, and reflect back
in the main blue, yellow, and green to our eyes. Hence it is incumbent
on those who are studying colour, and who are interested in the purity
and permanency of colour, to comprehend at least the principles of
that science of light which tells of the action of light upon various
bodies that are used as pigments in painting.

If we put together two substances one of which destroys or modifies
the chemical condition or state of the other, then certainly one of
those substances, and very probably both, will lose the colour which it
had before it came into contact with the other. It is therefore most
important that all engaged in the preparation and use of colours should
make a study of this science of light. Of almost equal value is a study
of the science of heat. We have seen what heat can do in changing the
conditions of a substance. To give another instance. The black sulphide
of mercury, after sublimation by heat, exhibits properties, imparted
to it by the heat, which it did not possess before, i. e. it can, by
trituration, be brought to display a red colour.

On showing the spectrum on a screen, if some solution of soda or other
sodium salt be held in the course of the light, almost all the coloured
rays but one will be cut off, and a little band is seen in the yellow
part of the spectrum. This is because the sodium flame is almost
“monochromatic,” or single-lined: it cuts off all the colours but the
yellow. Again, if metallic thallium is held in the flame, the only band
remaining in the spectrum will be the green; and if a lithium salt, the
only surviving colour will be red.

=Pigments.=--The term “pigments” is applied to those colouring matters
which are mixed in a powdery form with oil or other vehicle for the
purpose of painting. They differ in this respect from the dyestuffs,
which are always employed in solution. A very large proportion of
the pigments in common use are derived from the mineral kingdom, the
most notable exceptions being found in the blacks and lakes. All
pigments are required to possess “body,” or density and opacity; to be
insoluble in water and most other solvents, except the stronger mineral
acids; and to be inert, or incapable of exercising chemical or other
influence on each other or on the vehicle or drier with which they are
mixed prior to use. They may be conveniently classified according to
their colours in the first place, reserving the consideration of their
preparation for use for a later chapter. The chief classes are Blacks,
Blues, Browns, Greens, Reds, Whites, and Yellows.

CHAPTER II.

BLACKS.

All the black pigments in use owe their colour to carbon, and all are
produced by artificial means, no natural form of carbon possessing the
requisite qualities.

Several manufactured carbonaceous substances are known in commerce
under the generic name of “Blacks.” The most important of these are
animal-black, bone-black, Frankfort-black, ivory-black, and lamp-black.
They are usually obtained by carbonising organic matter, particularly
bones, in closed vessels or crucibles, or by collecting the soot formed
by the combustion of oily, resinous, and bituminous substances. Other
blacks than those enumerated are manufactured, but only on so small a
scale as to be of no commercial importance.

Carbon, lamp, and vegetable blacks consist almost entirely of carbon,
containing usually from 98 to 99½ per cent. of that substance, the
residue consisting of a little ash, water, and occasionally unburnt
oil. Bone and ivory blacks, on the other hand, are chiefly composed of
mineral matter, which may amount to 65 or 75 per cent. and is mainly
represented by phosphate of lime. Their actual colouring matter, the
carbon, only constitutes 15 to 30 per cent. of the mass. The balance is
water and unburnt animal tissue. Blacks prepared from animal matters
other than bone and ivory carry 40 to 80 per cent. of carbon, and their
mineral matter is generally in the form of carbonates of lime and of
the alkalies.

The principal impurity to be watchful of in the vegetable and lamp
blacks is a small quantity of oily matter which may seriously
interfere with their drying qualities. They should leave very
little ash after being burned in a crucible. Bone and ivory blacks
are sometimes valued as much for their mineral matter as for their
colouring matter. The proportion of this mineral matter is ascertained
by heating a certain weight of the black to red heat in a crucible till
every trace of black has disappeared, and then weighing the residue.
The residue should next be boiled in strong hydrochloric acid till
it is dissolved; if there is any which will not dissolve it is most
probably barytes, which has been added as an adulterant and to make
the black weigh heavy. When the solution is complete, the addition
of ammonia will throw down a precipitate of phosphate of lime, which
should equal 60 to 70 per cent. of the original weight of mineral
matter. If much less than this, it is likely that whiting or gypsum
has been mixed with the pigment. As carbon is not acted upon by acids
or alkalies, it follows that all pure carbon blacks are in themselves
perfectly stable and permanent pigments, and that they exert no
influence on other pigments with which they may be mixed.

=Animal-black.=--This substance is almost identical with bone-black,
but is generally in a more finely divided state. Any animal refuse
matter may be used in its preparation, such as albumen, gelatine, horn
shavings, &c. These are subjected to dry distillation in an earthenware
retort. An inflammable gas is given off, together with much oily
matter, ammonia, and water, while a black carbonaceous mass is left
behind. This is washed with water and powdered in a mill, the product
being animal-black. It is largely used in the manufacture of paint,
printing ink, and blacking.

=Bone-black.=--When bones are heated in a retort or crucible, the
organic constituents are decomposed and carbonised. A mixture of
combustible gases is given off; some of these do not condense on
cooling, others condense in the form of a heavy oil, called bone-oil.
Also much water containing tarry water and ammoniacal salts in solution
passes over. The residue in the retort or crucible consists of finely
divided carbon, in intimate mixture with the inorganic constituents
of the bones: this mixture constitutes ordinary bone-black, or animal
charcoal, as it is sometimes called. The inorganic portion may, if
required, be removed by washing the residue in dilute hydrochloric acid.

The process, as worked on the large scale, is carried on in different
ways, according as it is desired to collect the volatile condensable
portion of the distillate, or to allow it to escape. In the latter
case, when it is required to obtain only bone-black, the apparatus
employed is of a very simple nature, and the amount of fuel needed
is comparatively small. The carbonisation is effected in fire-clay
crucibles, 16 in. high and 12 in. diameter. These are to be preferred
to crucibles made of iron, which were much used at one time, since they
do not lose their round form when subjected to a high temperature; in
consequence of this, they fit more closely together in the furnace,
less air can penetrate, and therefore less of the charcoal is consumed
by oxidation. The furnace is an ordinary flat hearth, having a
superficial area of about 40 square yards, and is covered in with a
flat arch, all of brickwork. The fireplace is situate in the middle of
the hearth; the crucibles are introduced through doors in the front,
which are bricked up when the furnace is filled; each furnace holds
eighteen crucibles. The crucibles, filled with the coarsely broken
bones, are covered with a lid luted on with clay. To economise fuel,
the furnaces should be in a row, and placed back to back.

The arrangement of the furnace and pots is shown in Figs. 1 and 2. A is
the fireplace; B, the crucibles, eighteen in number, spread over the
floor of the furnace in a single layer; _c_, _d_, _e_, and _f_ are the
flues for conducting away the heated gases arising from the calcination
of the bones, as well as the waste heat itself; the last portion of the
flue is fitted with a damper _g_. The furnaces are intended to be built
in fours, back to back, the waste heat serving in a great measure to
conduct the operation of the revivifying apparatus placed in the centre
of the group, and marked C.

[Illustration: Figs. 1 and 2.--BONE-BLACK FURNACE.]

When the furnace is filled and the doors are bricked up, the heat is
slowly raised to redness, at which point it is kept for six or eight
hours. The combustible gases are evolved and consumed in the furnace
as the bones begin to decompose, and by this means so much heat is
produced that only a small quantity of fuel is needed to maintain the
required temperature. When the carbonisation is complete, the doors are
taken down and the crucibles are removed to cool, their places being
immediately filled with fresh ones. The heat must be kept as uniform
as possible throughout the process: if it be not sufficiently high,
the bone-black will contain a portion of undecomposed organic matter,
which renders it quite unfit for use; if, on the other hand, the
temperature be raised too high, the bone-black will become dense and
compact, whereby its efficacy as a decoloriser is much reduced. When
the charcoal in the crucible has become perfectly cool, it is removed
and crushed. When required for decolorising or deodorising purposes, it
is only roughly broken up into small lumps, in which form it is most
readily applicable. The crushing is effected by means of two grooved
cylinders, consisting of toothed discs, alternately 10 and 12 in. in
diameter. These are so placed that the 10-in. discs of one cylinder are
opposite the 12-in. discs of the other, and thus, in revolving, the
carbonised bones are crushed to fragments between them, but are not
reduced to powder. They are passed successively through six of these
mills, the cylinders of each couple being nearer to each other than
the last. Finally the crushed bones are carefully sieved; the powder
is placed apart from the lumps, again passed through finer sieves, and
sorted out into different sizes.

A furnace such as that described above will carbonise four charges of
bones in one day, each charge being more than half a ton in weight.
With careful work, the bones will yield 60 per cent. of bone-black, or
more than one ton daily.

If it be required to condense the volatile gaseous products of the
carbonisation, this process is conducted in retorts similar to those
used in the manufacture of acetic acid from wood: these are so arranged
that the whole of the gaseous products are condensed and collected.
The aqueous portion of the distillate is usually evaporated down to
obtain salts of ammonia; the uncondensable gases may be employed for
illuminating purposes. The manufacture of bone-black is usually carried
on in the neighbourhood of large towns, where a good supply of bones
may be readily obtained.

Ordinary bone-black has about the following composition: Phosphate and
carbonate of lime, and sulphide or oxide of iron, 88 parts; charcoal,
containing a small quantity of nitrogenous matter, 10 parts; silicated
carbide of iron, 2 parts. The decolorising properties of bone-black are
due solely to the presence of the charcoal.

When intended for use as a deodoriser or decoloriser, bone-black should
be kept carefully excluded from the air, for by exposure it loses this
power to a great extent, and becomes almost inert. That which has been
freshly burned is therefore best for these purposes.

The cost of production of bone-black may be calculated as follows:--

£ _s._ _d._
4 tons fat bones at 4_s._
per cwt 16 0 0
27½ bushels coals 1 3 9
2 firemen 0 4 9
4 workmen 0 8 0
1 carman 0 2 4
2 horses 0 5 7
Breaking up the bones 1 5 4
Rent and taxes 0 8 0
Interest, repairs, and
wear and tear 0 7 2
Contingencies and transports 0 2 4
-------------
£20 7 3

Produce:--

Black, 60 per cent., say 38 cwt. in grains, at
14_s._ 3_d._ 13 10 9
10 cwt. fine, at 5_s._ 6_d._ 1 7 8
Fat, 6 per cent., say 5 cwt., at 31_s._ 8_d._ 7 18 4
---------
£22 16 9 22 16 9
--------
Profit £2 9 6

Bone-black never has the depth or brilliancy of lamp-black, but it
mixes well with either water or oil, and though a slow drier as an oil
paint, is permanent and not high priced.

=Frankfort-black or Drop-black.=--This is a black powder obtained
from dried vine-twigs carbonised to a full black and then ground very
fine. On a large scale it is prepared from a mixture of vine-twigs,
wine-lees, peach-stones, bone-shavings, and ivory refuse. It varies
in shade according as the animal or vegetable charcoal is in excess;
when the latter predominates, the powder is of a bluish colour; but
when there is an excess of animal charcoal, it has a brownish tinge.
It is customary to wash the powder well when first made, in order to
remove any soluble inorganic impurities. The finest Frankfort-black
is probably the soot obtained from the combustion of the materials
mentioned above. It makes an excellent pigment, and is extensively used
by copperplate engravers in the preparation of their ink. Drop-black
is simply Frankfort-black ground exceedingly fine, mixed with a little
glue water, and dried in pear-shaped drops for sale.

=Ivory-black.=--Ivory-black is a beautiful black pigment prepared by
carbonising waste fragments and turnings of ivory. These are exposed
to a red heat for some hours in crucibles, great care being taken
to avoid overheating or burning. When quite cold, the crucibles are
opened, and the contents are pulverised, the richest coloured fragments
being kept apart for the best quality. The powder is then levigated
on a porphyry slab, washed well with hot water on a filter, and dried
in an oven at a temperature not exceeding 212° F. The product is of a
very beautiful velvety black colour, superior even to that obtained
from peach-kernels, and quite free from the reddish tinge which so
often characterises bone-black. Ivory-black, like Frankfort-black, is
employed by copperplate printers in the preparation of their ink. Mixed
with white lead, it affords a rich pearl-grey pigment.

=Lamp-black.=--Lamp-black is an exceedingly light, dull-black powder,
formed by the imperfect combustion of oils, fats, resins, &c. It may
be prepared on a small scale by suspending a small tin-plate funnel
over the flame of a lamp fed with oil, tallow, or crude naphtha, the
wick being so arranged that it shall burn with a large and smoky flame.
Dense masses of this light carbonaceous matter gradually collect in
the funnel, and may be removed from time to time. The funnel should be
furnished with a metal tube to convey the gases away from the room, but
no solder must be used in making the connections.

[Illustration: Figs. 3 and 4.--APPARATUS FOR MAKING
LAMP-BLACK.]

An especially fine quality of lamp-black is obtained from bone-oil,
deprived of the ammonia with which it is always contaminated. It is
manufactured on a commercial scale by means of the apparatus shown
in Figs. 3 and 4. The oil is contained in the lamp A and kept at a
constant level by means of the globular vessel B, which is also filled
with oil and inverted over A. The oil flows from the lamp into the
tube C, which is bent upwards at the farther extremity on a level with
the oil in the lamp. A cotton wick is supplied to the bent end of the
tube, as well as a little spout D, for conducting away any oil that
may overflow into the receptacle E placed beneath. A conical hood _a_
surrounds the flame of the lamp and terminates in a tube _b_, through
which are conveyed the sooty products of the combustion of the oil into
the wide lateral tube _c_, arranged to accommodate the smoke from about
a dozen such lamps placed at intervals of about 6 feet, as indicated in
the figures. The effect of this wide tube _c_ is not only to cool the
smoke, but also to collect the water and other liquids condensed. The
smoke and vapours pass hence into _d_, the first of a series of sacks
made of closely woven linen, about 10 or 12 feet long and 3 feet in
diameter, closed at the bottom with a trap or slide _e_, and formed at
the upper and lower ends of sheet-copper tubing made funnel-shaped. The
upper one of these is prolonged into an additional pipe _f_, by means
of which the smoke arrives at the second sack _g_ in the series, thence
finding its way to the third, and so on till the last sack of the row
is reached. In connection with the last sack of each row is placed a
horizontal flue F, in which are arranged frames covered with wire gauze
and mounted on hinges. Their purpose is to retain the small remaining
portions of lamp-black passing out with the smoke from the sacks. The
meshes of the gauze are constantly getting filled up with soot, which
necessitates a periodical checking of the draught for its removal. This
is done by means of the rod G, which, when raised and allowed to fall
suddenly, jerks the accumulated mass off the gauze. The current of
air passing through the entire apparatus can be regulated by a damper
placed at the entrance to the chimney in which the flue F embouches.
At regular intervals, the mouthpieces in the lower ends of the sacks
are removed, and their contents are shaken out separately and collected
according to their various qualities. That gathered from the first sack
in each row should always be kept apart from the remainder, as it is
much contaminated by the presence of resinous and tarry matters.

[Illustration: Fig. 5.--APPARATUS FOR MAKING LAMP-BLACK.]

The old-fashioned method of preparing lamp-black from the incomplete
combustion of gas tar is conducted in an apparatus resembling that
shown in Fig. 5. The furnace _a_, lined with fire-brick, contains a
kettle _b_, and is surmounted by a large thick cast-iron hood _c_,
communicating with a stone or brick condensing chamber, divided
by means of perforated partition walls into three unequal sized
compartments _d_, _e_, _f_, wherein the black is deposited. A chimney
_g_ delivers uncondensed vapours into the atmosphere. In working, the
furnace is first brought to a red heat, then the kettle _b_, charged
with tar, is introduced. As a charge is finished, more tar is added,
with occasional stirring, till the kettle becomes inconveniently full
of residue, when it is withdrawn and a fresh one replaces it. The
residue is chipped out and used as fuel. The black is removed weekly
through the door _h_. It is of good quality and colour so long as the
combustion is conducted with a minimum of air, admission of which is
controlled at the furnace. The yield is about 25 per cent. of the
weight of the tar; and one furnace should treat a ton of tar in a week.
One workman can manage several furnaces.

An improved process has been introduced by Martin and Grafton for the
preparation of lamp-black from coal-tar, which affords a very good
product. The coal-tar is first stirred up energetically with lime-water
in any convenient vessel, after which the mixture is allowed to stand
until the coal-tar has subsided to the bottom, when the lime-water is
drawn off. The tar is then well washed by decantation with hot water,
and rectified in the ordinary naphtha still. Afterwards it is run into
a long iron cylinder, which is placed over a furnace, and supplied
with numerous large burners. Each burner has a metal funnel placed
immediately above it, connected with a cast-iron pipe, into which all
the fumes from each burner are conducted. The naphtha in the cylinder
is heated almost to the boiling point by the furnace beneath. A series
of smaller pipes lead away the fumes from the main pipe into a row of
chambers, and thence into a series of large canvas bags, placed side
by side, and connected alternately at top and bottom. The bags vary
in number from fifty to eighty, the last one being left open to allow
the smoke to escape, after traversing some 400 yards since leaving the
burners. The best quality of lamp-black is found in the last bags, that
near the furnace being much coarser and less pure. The bags are emptied
whenever they contain a sufficient quantity.

The process employed in Germany for the manufacture of lamp-black is
to conduct the products of the combustion of any resinous matter in a
furnace into a long flue, at the end of which is placed a loose hood,
made of some woollen material, and suspended by a rope and pulley. The
lamp-black collects in this hood, and, when a sufficient quantity has
accumulated, is shaken down and removed. In this manner about 6 cwt. of
lamp-black may be collected in twenty-four hours.

One form of the apparatus is shown in Fig. 6. The circular structure
_a_ is lined inside with hanging cloths upon which the black can
condense, and is covered with a conical roof from which depends a
movable sheet-iron cone _b_, perforated at its apex to give egress to a
current of air. This cone _b_ is supported by a rope _g_ passing over a
pulley _c_ and accessible from the outside. A fireplace _d_, containing
a small iron dish _e_ for holding the resin, is built against one of
the side walls of the structure in such a manner that it can be fired
externally. The rate of combustion is regulated by a small sliding
damper on the door of the fireplace. When the black has accumulated in
the chamber _a_ to such an extent that operations must be suspended,
the fire is let out, and the chamber is left to cool entirely, so that
the black may not ignite on contact with the air. The cone _b_ is then
lowered, and in its descent scrapes the walls of the chamber _a_ and
causes the black to collect on the floor, whence it is removed through
an iron door _f_ which at other times is kept tightly luted.

[Illustration: Fig. 6.--APPARATUS FOR MAKING LAMP-BLACK.]

In England, an inferior variety is sometimes obtained from the flues of
coke-ovens. That known as _Russian lamp-black_ is made by burning chips
of resinous deal or pine wood, and collecting the soot formed; but it
is objectionable, owing to its liability to take fire spontaneously
when left for a long time moistened with oil.

A modified form of apparatus has been introduced by Thalwitzer, a
German manufacturer, and is shown in Figs. 7 and 8. A vertical tube is
provided at its upper end with a funnel, into which cooling water is
poured and flows out through openings in the tube immediately above a
circular plate of thin cast or wrought iron arranged horizontally and

[Illustration: Figs. 7 and 8.--THALWITZER’S LAMP-BLACK
APPARATUS.]

secured at its centre to the tube. Round the periphery of this plate
is a vertical rim of tin plate, at the top of which is a pipe through
which the cooling water runs into a gutter round the top of the
cylindrical casing, the water being carried off from this gutter by
a pipe. The vertical tube is carried near its upper end in a bearing,
and at that part is attached a worm-wheel geared into it by a worm
driven by any suitable power. At the underside of the circular plate is
fixed a scraper, the edge of which is formed with a strip of leather in
contact with the lower surface of the plate. Opposite the scraper, at
the bottom of the casing, is a burning lamp, which sucks up the oil for
its consumption by a flat wide wick.

The operation is as follows:--The vertical tube is caused to revolve
by the action of the worm-wheel, the circular plate thereby receiving
a slow rotary movement; and a small stream of water being poured into
the funnel at the top of the tube, this water passes down the latter
and through the openings on to the circular plate, which is thus kept
cool. The burning lamp filled with paraffin or other oil is brought as
near to the circular plate as is necessary for the cooling of the flame
and the most perfect extraction of the carbon, which, in the form of
soot, attaches itself readily to the plate, owing to its coldness and
to the condensation of the steam produced. The revolving plate presents
continually to the flames a new and clean surface, in consequence of
the lamp-black being scraped away by the scraper as soon as deposited,
and brought away through a pipe or shoot into a collecting barrel.

The apparatus as shown in Figs. 7 and 8 consists of a round metal
plate A, provided with a flange _a_, and fixed on a vertical shaft _b_
supported by the bearing B, and carrying at its upper end a worm wheel
_d_ set in motion by a worm. The plate A is cooled by water admitted
through a pipe _g_, and the flange _a_ is provided with a discharge
pipe _h_, through which the cooling water runs into the groove D,
surrounding the whole apparatus. Underneath the plate A a number of
lamps J are applied, which are fed with oil by a common pipe _l_. H is
an oblique scratcher or blade, the working edge of which is formed by a
strip of leather, and touches the lower surface of the plate A.

For manufacturing lamp-black, a slow rotary motion is imparted to the
apparatus by means of the worm and worm-wheel, and a slight current
of water is directed upon the plate A through the pipe _g_. The lamps
J, filled with paraffin oil derived from lignite, or with any other
suitable oil, are ignited and approached to the plate A as far as
is necessary for cooling the flame, so as to deposit the greatest
possible quantity of black. The latter adheres to the cold surface of
the plate, which is also kept damp by the aqueous vapour formed during
the combustion. The revolution of the plate serves to bring the flame
continually into contact with new and clean portions of the plate, the
black being continually scraped off by the blade or scraper placed
opposite the flames, and conducted through a channel into a collecting
trough.

There is a risk of overburning, causing a grey tint and a hard and
granular texture.

A variety of lamp-black known as “carbon black” or “gas black,” has
of late years assumed an important position among black pigments. It
is produced in considerable quantities in the United States by the
combustion of the natural gas issuing from the earth in the mineral oil
regions. The soot arising from the imperfect combustion of the gaseous
hydrocarbon is made to deposit itself on cooled iron surfaces. These at
first were made stationary, but now take the form of revolving discs or
cylinders, which are automatically cleansed of the black as fast as it
is deposited. This type of lamp-black is remarkably free from mineral
impurities and unburned oil, and of a full colour.

An improved lamp-black kiln has been introduced in which the use of
water is dispensed with. It is shown in Figs. 9 and 10. The furnace A,
which is preferably built double, as shown, is constructed of brick
lined with firebrick, with a rear wall _a_ that divides the furnace
room from the condensing room, side walls _b_, front _c_, and central
dividing wall _d_, that divides the furnace into two long and narrow
fire

[Illustration: Figs. 9 and 10.--AMERICAN LAMP-BLACK KILN.]

spaces. The bottom of the fire spaces _e_ is formed by a sheet iron
plate _f_ that is supported by the walls, and the space below plate _f_
serves as an air space through which air circulates by openings _g_
in the front and side walls, this circulation of air tending to keep
the plate _f_ cool. The rear of the fire space _e_ extends upward and
communicates by an opening _h_ through the wall with the condensing
room. In the front wall _c_ is an opening to each fire space _e_ and
a door _i_ to each opening. The oil or other liquid is supplied by
pipes _k_ that enter from the outside near the rear of the fire spaces.
The outer end of each pipe _k_ is fitted with a cup-shaped receptacle
_l_, into which the oil will run from the vertical branch of the main
supply pipe _m_, so that the amount of oil running into each pipe
_k_ may be observed, and regulated by a cock. The pipe _m_ feeds the
oil to one or more furnaces, the supply of material to each furnace
being separately regulated. In the fire spaces beneath pipes _k_ are
placed shallow cast iron drip pans _o_ to receive the oil, and the oil
running in faster than it will burn will drop while on fire into the
pans _o_, and be spattered into small particles. These pans are changed
frequently, access to them being obtained by doors _i_. A slide _p_ is
provided in each door _i_ to allow of ventilation when required. The
slides and doors should close air-tight. By constructing the fire space
_e_ long and narrow, the plate _f_ is more readily kept cool, and the
space in front of the point of combustion renders the smoke less liable
to escape by the doors. The products of combustion pass through the
opening _h_ to the condensing room, which is lathed and plastered, and
if the room is sufficiently large a number of furnaces may be fitted to
discharge into the same room. This furnace is especially adapted for
burning dead oil; but by using burners of suitable construction other
oils may be burned, and a superior quality of lamp-black made from
mitigated spirits.

A very large proportion of the lamp-black now made is derived from the
combustion of creosote or anthracene oils from coal tar, or of the
residues of shale-oil distillation. The form of combustion chamber
varies in different works, but is typified by the following rough
sketch of that in use at the Stampshaw Chemical Works (Fig. 11).

[Illustration: Fig. 11.--_Apparatus for making Lamp-black from Creosote
or Shale Oil._]

At these works a horizontal brick flue _a_ about 18 inches square and
about 10 feet long is provided. At one end it enters the black-house
_b_, and is here provided with a damper _c_ to shut it off when not
working. The other end opens to the air, and here is a sliding door
_d_ which, when shut down, leaves an opening round a small pipe _e_,
which enters in this situation from a main pipe that conveys oil in a
similar manner to four burners of this description placed side by side.
At the bottom of the flue is an iron tray _f_ to catch any liquid that
falls from the tube, and in this tray the oil is burned. The burning of
oil in one of these flues is not allowed to go on for more than three
hours, and, when the combustion is over, the communication with the
black-house is closed, the entrance door of the flue is opened, and the
cover is taken off the chimney _g_ so that the flue may become cooled,
and another flue is taken into use.

The black-house is a brick chamber into which the smoke passes, and
where it deposits its sooty particles. In some works there is only
one undivided chamber; in other works there are more than one, and
the chambers communicate by flues through which the smoke passes from
one to another. At other works the chamber is divided by vertical
partitions, springing alternately from the two ends, so as to
constitute one high zigzag flue, along which the smoke must travel
to its outlet from the black-house. This chamber must needs have an
opening somewhere to the outer air. The opening is sometimes a small
chimney in the roof, and sometimes a short louvre tower. This is
necessary to produce a trifling draught, just enough to carry the smoke
into the chamber and no more.

In some works, the black from the black-house is also calcined, the
object of the “calcination” being to get rid of all greasiness, a point
of great importance when the lamp-black is to be used for making fine
pigment. This process is conducted in circular iron pans, usually about
2¼ feet high and 2¼ feet diameter, which are provided with removable
iron covers. A pan of this size will hold about 2 lb. of lamp-black. A
bowlful is first put in and lighted by a red-hot iron; more and more is
added from time to time as the ignition proceeds. When the pan, being
full, leaves off smoking, the calcination is known to be complete, and
the pan is then covered and its contents are allowed to cool. The loss
undergone in this process is about 25 per cent. The smoke which comes
off is acrid and very irritating to the eyes, like that proceeding from
boiling oil, and it is difficult for a person unaccustomed to it to
remain many minutes in the chamber where calcining is going on. This
process is sometimes conducted within a chamber, but frequently under a
shed or even in a building freely open to the air.

There are three sources from which nuisance may arise in lamp-black
making: 1. The smoke which issues from the chimney of the black-house,
small as it sometimes is, often constitutes a nuisance to near
neighbours; but the nuisance is not a very serious one, and it does not
extend very far from the works, never to a greater distance than about
50 yards. The odour, even when but little smoke escapes, is oppressive
and suffocating in character, and resembles that diffused in a room
by a smoking table-lamp. It occasions headache, but is not otherwise
injurious to health. 2. A similar nuisance of suffocating smoke
sometimes proceeds from the burners, but this is when they are leaky or
when there is a deficiency of draught through the black-house, or when
the doors of the burning chambers do not shut closely, and when there
is much wind blowing past them. This nuisance chiefly occurs when the
burners are open to the air and merely protected by an open shed. 3.
The escape of acrolein and other offensive vapours from the calcining
house.

The best mode of preventing nuisance from the black-house is so to
elongate the chamber as to give abundant opportunity for the soot to
deposit in the course of the smoke along it to the outlet, and by
taking means to consume by fire what little smoke escapes deposition. A
most effectual arrangement for the accomplishment of these ends is to
have a black-house 150 feet long, and so divided by partitions within
as to cause the smoke to traverse a distance of altogether 500 feet
before it finds an exit; the exit from the chamber communicating with a
fire, in which the last of the smoke is consumed, and which serves to
assist in regulating the draught through the chamber.

The regulation of the draught through the burner and black chamber is
of importance in order to avoid the escape of smoke from the burners.
If the draught be too great, too much black is lost from the chamber,
but if, on the other hand, it be too little, the smoke instead of
passing into the chamber will come out into the works and create a
nuisance, especially where the burners are erected in the open air,
under circumstances in which variation in the force of the wind cannot
fail to interfere with due regulation of draught. This part of the
manufacture should be conducted within a building of some sort.

The best mode of preventing nuisance from calcination is in operation
at Shackell & Edwards’ works, in Hornsey Road, Islington. At these
works the black is calcined in a chamber 20 feet square and 25 feet
in greatest height, with a paved floor and arched roof. In the centre
of the roof is the opening where a fire was formerly placed, but which
is now closed by a sky-light, capable of being raised. The calcining
pots are ranged round this chamber, and a fan, employed to draw off
the vapours from the oil-boiling pans, is further utilised to draw off
also, from the upper part of the calcining-house, the vapours arising
from the calcination, and to drive them into the boiler fire, where
they are consumed. Calcination should always be conducted in a closed
building duly ventilated so as not to create nuisance.

The transport of lamp-black is effected in barrels or bags; when in the
latter, these should be previously soaked in water containing some clay
in suspension, which stops up the pores of the sacking, and thereby
prevents loss.

The particular virtue of lamp-black as a pigment lies in its state
of extremely fine division, which could not possibly be attained by
artificial means; this quality renders it invaluable as the basis of
black pigments, all of which contain it in a greater or less quantity.
Indian ink and printers’ ink are also composed principally of this
substance.

=Unimportant Blacks.=--In addition to the recognised blacks already
noticed there are a number of other sources of black pigment which
have been drawn upon to a limited extent, or have been suggested
as substitutes for the standard articles. They only merit a short
description.

_Aniline black_ is prepared by adding an acidified (sulphuric) solution
of bichromate of potash to an aqueous solution of hydrochlorate of
aniline, and washing the precipitate. The cost is prohibitive.

_Candle black_ is candle smoke condensed on a cold plate.

_Charcoal black_ is finely-ground wood charcoal.

_Coal black_ has been suggested by grinding coal, but lacks the
requisite qualities of a pigment.

_Cork black_ is a very fine pigment prepared by calcining cork refuse.
Limited supply.

_German black_ is Frankfort black.

_Iron black_ is ground black sulphide of iron.

_Lead black_ is prepared by boiling lead fume in sulphide of soda
solution. It would probably be unstable on account of oxidation.

_Manganese black_ is ground oxide of manganese. It is costly, and dries
too quickly.

_Prussian black_ is calcined Prussian blue. It is not of a good colour,
nor economical.

_Prussiate black_ is the carbonaceous residue from making yellow
prussiate of potash. Used chiefly for decolorising syrups, &c.

_Spanish black_ is cork black.

_Tannin black_ is proposed to be made by exhausting the tannin from
refuse leather and tanning agents, and adding alum and sulphate of
iron. The colour is blue-black, weak, and unstable.

CHAPTER III.

BLUES.

=Cobalt Blues.=--Some of the compounds of cobalt with alumina,
phosphoric acid, silica, and tin, are remarkable for possessing a fine
blue colour of great permanency and indestructibility, and still find a
limited application. They are chiefly as follows:--

Cœruleum--a mixture of the oxides of cobalt and tin.
Cobalt blue--a mixture of the oxides of cobalt and alumina.
Smalts--a double silicate of cobalt and potash.

CŒRULEUM.--This is a light-blue slightly greenish colour, with
no purple tendency in artificial light. It is non-granular, covers
well, mixes with water or oil, and is a good artists’ colour for sky
effects. It is permanent in strong sunlight and impure atmosphere, and
resists acids and alkalies at normal temperatures. Hot hydrochloric
acid dissolves it, and addition of water to the pale blue solution
produces a violet red; evaporation to dryness restores the original
pigment. The green tint of a nitric acid solution is due to iron and
nickel impurites. Dilute sulphuric acid causes partial decomposition
of cœruleum, but it is proof against caustic potash, acetic acid, and
concentrated sulphuric acid. Its composition is given as

Cobalt oxide 18·66
Tin oxide 49·66
Silica and sulphate of lime 31·68
------
100·00

There are several methods of preparing cœruleum:--

(1) A solution of stannate of potash is added to one of cobalt. A blue
precipitate is thrown down, which, on washing, becomes first light-red
and then brown. When calcined at a white heat it assumes a blue colour.

(2) A solution of stannate of soda is mixed with a solution of nitrate
of cobalt, and the resulting precipitate calcined to bright redness
forms a blue pigment.

(3) Solutions of cobalt and tin are mixed and precipitated by soda, the
precipitate washed free from soda being calcined as in all the other
cases. The silicate of soda is the most satisfactory sodium salt for a
precipitant.

COBALT BLUE.--This rich pure blue pigment is not alone
permanent, but actually develops its full intensity only after exposure
to the air. With age, however, it acquires a greenish tendency,
and in artificial light it inclines to a violet tint. It is proof
against acids and alkalies, and mixes particularly well with water.
In combination with other pigments it is unaltered and has no effect
on them. Its tones are different from those of ultramarine. It slowly
decomposes when heated in strong sulphuric acid, yielding a violet
solution and a white precipitate, which latter dissolves and affords a
blue liquid on dilution with water. It consists principally of about 80
per cent. alumina, and 15 per cent. oxide of cobalt.

There are several ways of preparing it:--

(1) By Thénard’s original process, roasted cobalt, from Tunaberg,
Sweden, is dissolved under heat in an excess of nitric acid. The
solution, evaporated nearly to dryness, is boiled in water, and the
deposit of arseniate of iron is filtered out. Into the filtrate is
poured a solution of basic phosphate of soda, which throws down
a precipitate of basic phosphate of cobalt, varying in hue from
violet to pink. This precipitate is washed on a filter, and, while
still gelatinous, 1 lb. of it is intimately mixed with 8 lb. of
hydrated alumina, recently precipitated by ammonia from a solution of
potash-alum. The mass is first dried to brittleness and then calcined
in a covered clay vessel for half an hour at a cherry-red heat. The
resultant blue pigment is stored in glass receptacles.

The preparation of the gelatinous alumina is conducted as follows. The
potash-alum is dissolved in at least three times as much water as is
necessary, and is then precipitated by an abundant excess of ammonia,
with frequent stirring. When settled, the supernatant liquor is
siphoned off, and the precipitate is thoroughly washed several times on
a filter.

Thénard blue will vary in tint according to the proportions of
alumina used. A pure colour is obtained with 4-5 parts alumina to 1
of phosphate of cobalt; a greenish hue with equal parts of alumina
and cobalt salt; and almost any intermediate tone by varying the
proportions between these limits.

(2) To 16 parts of gelatinous alumina add 1 part of arseniate of
cobalt, obtained by precipitating the solution of cobalt by arseniate
of potash.

(3) A richer and more velvety blue is got by using oxide of cobalt and
substituting phosphate of lime for the alumina (Boullai-Marillac).

(4) Binder’s process is as follows:--Dissolve by boiling 6 lb. alum,
free from iron, in a leaden or earthenware vessel, and filter it into
a vat 5½ ft. high and 3 ft. across, one-third full of clean water.
Precipitate the alumina by solution of potash, fill up the vat with
water, settle, decant the clear liquor, and wash repeatedly till
barium chloride gives no precipitate. Dissolve ½ lb. sesquioxide
of cobalt in 1½ lb. hydrochloric acid at 22° B., and evaporate to
dryness. Dissolve the residue in 3 lb. hydrochloric acid, and pass
a stream of sulphuretted hydrogen through it, to throw down any
foreign metals. Filter clear, evaporate again to dryness, and dissolve
the residue in enough water to produce 4½-5 lb. of solution. Next
precipitate the cobalt solution (3 to 6 lb., according to depth of
tint required) by ammonia, avoiding excess. Wash the precipitate, and
add it to the water, holding the gelatinous alumina in suspension,
stirring thoroughly for ½ an hour. A reddish tint in the supernatant
liquor shows that some of the cobalt has been dissolved. Add a little
ammonia, and allow the precipitate to settle. Decant and add new waters
repeatedly. Finally collect on a fine filter cloth, drain, press, stove
dry, and calcine for 2-2½ hours at red heat in clay crucibles: then
cool, grind first in a mill and then on a slab, and sift.

SMALTS.--This pigment has not maintained its position in
competition with artificial ultramarine. Formerly it was very largely
used to correct the yellow tone of cottons, papers, and pottery. It has
a pale violet-blue tint, which, however, is not constant in artificial
light. Being a silicate it is very permanent, and proof against the
action of acids, alkalies, and sunlight, besides being inert when
mixed with other pigments. It can be used with either water or oil as
a medium, but is not a successful paint owing to its weak colouring
power. It is virtually a double silicate of cobalt and potash, or a
cobalt glass, containing a few impurities, of which the chief are
aluminium, iron, and lead oxides. The colour varies somewhat according
as these impurities fluctuate, and the finest ground sample is always
the palest. It is hardly ever adulterated, and the chief point to
secure is that it be ground to the finest possible degree.

Its manufacture is most extensively and successfully carried on in
Saxony. The raw materials used are cobalt speiss (an arsenide of cobalt
and iron), potash, and sand. The ore is broken up into convenient sized
pieces and roasted at red heat in a reverberatory furnace provided with
a tall shaft for discharging the sulphurous and arsenical fumes at a
high altitude. When the evolution of these fumes has ceased and the
mass begins to assume a pasty consistence, the roasted ore is removed
from the furnace, cooled, reduced to a fine pulverulent condition (then
known as “zaffre”) and passed through a silken sieve. Should it be
necessary,

[Illustration: Fig. 12.--FURNACE FOR ROASTING COBALT ORES.]

the cobalt ore is first spalled and hand-picked to remove the ores
of foreign metals which are associated with it; and then reduced to
a very fine state in an edge runner or mortar mill, and freed from
earthy impurities by washing. The concentrated ore is then dried and
dead-roasted in small charges at a time (about 4 cwt.) in a specially
designed reverberatory furnace such as shown in Fig. 12, of which _a_
is the hearth on which the ore is spread; _b_, the fireplace, the
products of combustion from which pass over the ore on the hearth, and
thence into the flues _c_, which repeatedly circle round the furnace
so as to provide abundant opportunity for the arsenious oxide derived
from the combustion (oxidation) of the arsenic in the ore to condense;
this highly poisonous arsenious oxide is collected in a solid form from
the flues at convenient intervals by means of the doors _d_. The ore
is charged and discharged at the door _e_. The roasting should not be
carried to such a point that the whole of the sulphur and arsenic are
removed when making smalts, as by leaving a portion of these substances
in the ore at this stage, the ultimate purification is better
accomplished.

The next stage is to fuse the roasted ore with potash and silica so
as to form a blue glass. The proportions in which the ingredients are
mixed depend upon the depth of colour in the zaffre operated upon and
the tint desired in the finished smalts; hence it is always determined
by a preliminary experiment, and is then most carefully adhered to,
each material being accurately weighed out. Only the best potash can
be used, as it must be quite free from soda, and iron or other metal;
the effect of soda is to render the blue greenish tinted. Quartz
affords the requisite silica, and is hand-picked to ensure freedom from
alumina, iron, and lime, which import dullness into the colour, and
then ground to a fine powder in an edge runner mill. The duly weighed
quantities of the several ingredients are intimately mixed in wooden or
cement lined vessels, so as to preclude the possibility of any metallic
iron finding its way in; and as a further protection against this risk
a little white arsenic is often added so that the iron may be carried
down in the regulus which is formed during the fusion in the crucible.

These crucibles are of refractory earthenware quite free from lime,
and measure about 18 inches across at top, gradually diminishing to 14
inches at bottom, so that an ordinary charge is about ¾ cwt. They are
placed in rows in a furnace which generally bears a close resemblance
to a glass furnace, the operation being very similar. The form of
furnace common in Saxony, where most of the smalts is made, is shown in
Fig. 13. By means of a series of openings a in the walls of the furnace
the pots _b_ are introduced on to the hearth of the furnace, whereupon
the openings _a_ are bricked up again and remain closed during the
operation. The ingredients are charged into the pots _b_

[Illustration: Fig. 13.--FURNACE FOR MAKING SMALTS.]

by means of long iron ladles which are introduced through the small
square apertures _c_, which can be temporarily closed by a half-brick
or other simple article. The fire is then lit in the fireplace _d_,
and the products of combustion circulate around the pots _b_, and
finally escape at the orifices _e_ at the top of the furnace into
flues leading to the chimney _f_. After about 8 hours’ firing fusion
commences in the pots, whereupon the contents are thoroughly stirred by
rods inserted through the working holes _c_. The temperature is then
increased till a white heat is attained, this being necessary for the
formation of a glass. The fused mass is repeatedly sampled, and when
it has become quite homogeneous, and the regulus or speiss containing
the iron, antimony, bismuth, arsenic, copper, nickel, sulphur and other
impurities has completely separated itself and collected at the bottom
of the pots, the blue glass is ladled out and dropped at once into cold
water, by which it is disintegrated and rendered very brittle ready for
the subsequent grinding. The regulus is then drawn off from the pots
through holes provided for the purpose, and removed by the orifices
_g_, after which the pots are ready for another charge. They ordinarily
remain serviceable for about six months.

The grinding needs to be done with great thoroughness, and is
accomplished partly by stamps and partly by edge-runner mills in the
presence of water. The particles as reduced are floated off by the
water to a series of settling tanks communicating one with another.
The portion which settles in the first of the series is too coarse for
use, and is returned to the edge-runner for further grinding; while the
portion in the last of the series possesses such a weak colour that it
is rejected, or put into the crucible to undergo a second fusion. The
selected portions are dried ready for the consumer.

=Copper Blues.=--These form an unimportant class, being unstable
and not endowed with great colouring power. Their tint is pale and
greenish, and though opaque in water, they are not particularly so when
mixed with oil. Exposed to the action of sulphur or its compounds,
whether present as sulphuretted hydrogen in the air, or in combination
with a metal, forming another pigment with which they may be mixed,
copper blues undergo an important chemical change, the carbonates and
oxides of copper being converted into the sulphide, which is black.
Under the influence of heat too the blue carbonate will lose its
carbonic acid, and be turned into the black oxide. Ammonia and the
acids dissolve them, but other alkalies are resisted until heat is
applied. The chief kinds of copper blue are Bremen blue, cæruleum, lime
blue, mountain blue, Péligot’s blue, and blue verditer.

BREMEN BLUE.--This is a more or less pure hydrated oxide
of copper, varying in its qualities according to the method of
preparation. When made by precipitating a neutral salt of copper from
solution, it forms a dense and compact mass; whereas a porous and
pulverulent pigment results when basic and insoluble copper salts are
treated with alkalies.

(1) The foundation of the manufacture of this colour was waste copper
scrap, such as ship’s sheathing, from which, in various ways, was
prepared a basic chloride or oxy-chloride. Some of the methods adopted
were:--(_a_) 100 lb. scrap copper, 99 lb. powdered sulphate of potash,
and 100 lb. salt, moistened with clean water; (_b_) 100 lb. copper
fragments, 60 lb. salt, and 30 lb. diluted sulphuric acid (3 volumes
of water to 1 of acid); (_c_) a solution of copper oxide (scales) in
pure hydrochloric acid poured over the scrap copper. The method (_a_)
produces a chloride of copper which, in contact with more metal,
becomes a sub-chloride; this, absorbing more oxygen from the air, is
converted into the basic green “oxide” of the factories. By the (_b_)
process, the hydrochloric acid set free, and the atmospheric oxygen
produce the same result. In the (_c_) process a similar effect is
obtained.

It is of primary importance that no trace of this sub-chloride of
copper shall be allowed to remain, as it undergoes decomposition
by caustic alkalies, and throws down an orange-yellow sub-oxide of
copper. Hence it has sometimes been the practice to prepare the basic
oxy-chloride twelve months in advance, and to stir it frequently before
use. Complete oxidation, however, can be as satisfactorily accomplished
by alternately wetting and completely drying the mass.

An interesting phenomenon takes place during the transformation of
this green magma into a hydrated oxide of copper. On this magma being
introduced by degrees into a caustic potash or soda lye of about 22°
B., the thoroughly washed and dried product is exceedingly fine, with
great covering power, and deepens on addition of a little water. When
the magma is diluted with an equal volume of water, and the mixture at
once poured into an excess of caustic lye, with constant agitation, a
few minutes’ rest will suffice for the mass to assume a most compact
consistence. The colour thus produced, when washed and dried, is much
lighter in colour, and has less body. A blue derived from any of these
products is unsatisfactory as regards freshness and intensity of
colour; whereas by adding a small quantity of concentrated solution of
sulphate of copper to the magma before treating it with the alkaline
lye, apparently a highly basic sulphate of copper is produced which
deepens the colour.

A pigment with good body can be made in the following manner. To 100
lb. of the thick magma of basic oxychloride add a concentrated solution
of 7 lb. sulphate of copper, and then 40 lb. of a concentrated caustic
lye (32°-36° B,), with vigorous and rapid stirring, finally adding
about 150 lb. of caustic lye at 20° B. When the decomposition is quite
complete, the precipitate is carefully washed, passed through a fine
hair sieve, and filtered. Drying is effected at a low temperature, to
ensure that the hydrated state of the oxide is not changed; and the air
of the drying chamber must be free from acid or sulphuretted vapours.

(2) If neutral nitrate of copper be decomposed by an insufficiency
of potash carbonate solution, the flocculent precipitate of copper
carbonate resulting is by degrees transformed into a sub-nitrate of
copper, which goes down as a heavy green powder. On treating this
sub-nitrate with a potassic solution of zinc oxide, a dark-blue
coloured pigment is formed, which is apparently a zincate of copper
mixed with a very small proportion of a highly basic nitrate of
copper. Though very light it has great covering power. In practice the
manufacture is conducted as follows.

Calcine copper scales in a reverberatory or muffle furnace till the
sub-oxide is entirely converted into protoxide, or until it dissolves
in nitric acid without evolving red nitrous fumes. Heat is applied to
the solution of nitrate of copper, which is decomposed by addition of a
clear solution of potash carbonate. After effervescence has subsided,
small doses of potash carbonate solution are added till but little
undecomposed copper is left. This residue is recovered by decanting the
clear liquor, and repeatedly washing the green precipitate with small
quantities of clean water, collecting all the washings, and finally
precipitating by potash solution. On introducing the green carbonate of
copper into a new solution of copper nitrate, it is transformed into a
basic salt. Crystals of nitrate of potash are obtained by evaporating
the previous liquors.

To obtain an economic solution of zinc oxide, clippings of metallic
zinc are treated with a solution of caustic potash or soda in a
cast-iron vessel. The immediate result is a disengagement of hydrogen,
and saturation of the alkali with zinc oxide, which behaves as an acid.
The cleared liquor serves for decomposing the basic nitrate of copper.
The pigment produced is a handsome blue, and the potash liquor can be
evaporated down till it yields crystals of saltpetre. The economy of
this method lies in producing nitric acid cheaply from soda nitrate and
obtaining saltpetre as a bye-product.

(3) An inferior and cheaper pigment is made in the following manner.
To a solution of copper sulphate add one of barium or calcium chloride
till a white precipitate ceases to go down, and from the cleared blue
liquor all the copper is precipitated by addition of fresh milk of
lime. Usually the weight of quicklime required is 20 per cent. of the
copper sulphate. The settled, washed, and dried precipitate is the
pigment desired. The cleared barium or calcium chloride solution may be
used anew as a precipitant for the next batch.

CÆRULEUM.--This name has been given to the beautiful blue
pigment used in Egyptian and Pompeian mural paintings, and exhibiting
the same bright blue after 1000 years’ exposure to the weather as when
first used. Its composition has been given by Fouqué as approximately
63½ per cent. silica, 21 per cent. copper oxide, and 14 per cent.
calcium oxide, and he regards it as a double silicate of copper and
calcium. It is supposed to have been produced by fusing together
copper ore, sand and lime, but experiments have not yet resulted in a
successful imitation of the pigment, a difficulty being encountered
in the fact that if too high a temperature be permitted, destruction
of the blue colour ensues, and a green glass results instead. This is
unfortunate, as its remarkably bright and stable hue would make it very
popular if it could be manufactured at a moderate cost. It withstands
sulphuretted hydrogen, and even prolonged boiling with any of the acids
or alkalies.

LIME BLUE.--This pigment is essentially a mixture of hydrated
oxide of copper and calcium sulphate. It resists the action of alkalies
in the cold, but turns black when boiled in caustic soda, and is
completely soluble in hydrochloric acid. Ultramarine has largely, if
not entirely usurped its place. There are several ways of making lime
blue:--

1. Any soluble copper salt the acid of which will make a soluble salt
with lime is suitable, the only precaution necessary being that if in
the decomposition of the copper and lime salts, the combination of
the whole of the sulphuric acid with the lime is not attained, there
should be an excess of copper sulphate in the liquor rather than of
the lime salt. The resulting copper solution, containing very little
lime sulphate, is settled in a cool place for 24-36 hours, filtered,
and diluted with clean water down to about 18° B. Meantime a milk of
lime is prepared with very white and well-burned lime, slaked and mixed
with abundance of pure water, and kept stirred for a long time in a
lead-lined vat. After a short rest to permit sand, &c., to precipitate
itself, the milk is drawn off, and left to settle in lead-lined or
copper pans. The deposit is collected, ground in a mill where contact
with iron is impossible, and passed through a very fine sieve.

The mixture of lime and copper solution is made in the proportion
of 100 lb. dry lime with 175 dry copper salt, if the most intense
coloration is desired, but the proportion of lime may be much increased
without detriment to the pigment beyond lessening its intensity of
colour. After complete settlement of the precipitate, the clear liquor
is decanted; the pigment is carefully washed with clean soft water,
and drained on filter cloths till it is of a convenient consistence
forming a green paste. A definite weight of this paste calculated on
the dry pigment is taken for further incorporation, consequently it is
first necessary to ascertain how much water is in the paste. Usually
it amounts to 75 per cent., and on this basis 5 lb. of the paste are
stirred up with 1 gal. clean water in a lead-lined vat, with addition
of ½ lb. wet lime under constant agitation. Subsequently ¼ pint of
clear solution of best potash at 15° B. is well stirred in, and the
mixture is immediately taken to the mill and most thoroughly ground.

Further, for each 10 gal. of green paste is prepared a clear solution
of 1 lb. pure salammoniac in 2 gal. water and another solution of 2 lb.
copper sulphate in 2 gal. water. The liquid paste is drawn off from the
mill into a stoneware vessel, and the two solutions of salammoniac and
copper sulphate are immediately added. After complete agitation and
combination, the mixture is left for 4 or 5 days to settle, and turned
into a lead-lined vat, where it is repeatedly washed with clean waters
until turmeric paper is not discoloured.

(2) Precipitation of copper sulphate by excess of thin milk of lime in
the cold, followed by washing and drying, will give a lime blue which
will dry without turning black. Or 100 lb. of the copper sulphate may
be treated with a milk of lime prepared from 30 lb. quicklime and
addition of 12½ lb. salammoniac. When the liquor has become colourless,
the pigment is prepared from the precipitate; but the lime should be
ground after slaking, and the milk of lime left to stand for some days,
before use. The salammoniac seems to be essential to the production of
a pure full blue. Milk of lime poured drop by drop into the ammoniacal
copper solution gives a precipitate which redissolves on agitation,
and remains long in solution under heat, but finally throws down a
permanent precipitate, while the liquor on standing gives beautiful
blue crystals. From experiments it appears that out of seven atoms of
copper sulphate in the liquor, five are precipitated by milk of lime
and the last two are decomposed by ammonia. A greater proportion of
lime will produce a precipitate holding a certain quantity of less
valuable pigment. A smaller proportion of lime yields a finer coloured
and more crystalline pigment, because it crystallises partly in the
excess of solution, so that by incomplete decomposition a smaller
yield of superior pigment is obtained. The proportions necessary for
formation of the colour are 7 equivalents of copper sulphate, 5 of
lime, and 2 of ammonia, and if the 2 equivalents of ammonia be replaced
by 2 of lime and 2 of salammoniac, the proportions furnishing the
best colour will be 100 lb. copper sulphate, 24 lb. lime, and 22½ lb.
salammoniac.

Both caustic soda and caustic potash produce a fine blue precipitate
in a solution of ammoniacal copper sulphate with excess of ammonia,
but the liquor decolorises only on evaporation of the ammonia. The
precipitate becomes lighter-hued the more it is washed, and consists
of hydrated oxide of copper with a little carbonic acid; it does not
turn brown even when heated in presence of excess of potash or soda.
Moreover the presence of ammonia renders the hydrated oxide of copper
much more permanent. The composition of this pigment is given by
Gentele as 33½ per cent. copper oxide, 23½ sulphuric acid, 16 lime, and
the remainder water, &c.

MOUNTAIN BLUE OR AZURITE.--This natural blue pigment consists
essentially of a basic carbonate of copper, and is found in quartz
rocks in England, France, Bohemia, Hesse, Saxony, the Tyrol, and
Siberia. It affords a rich sky-blue paint of a permanent character,
but being comparatively costly is not largely employed. Its composition
is about 69 per cent. copper oxide, 25½ carbonic acid, and 5 water. The
only preparation needed is exceedingly fine grinding.

PÉLIGOT BLUE.--(1) Whereas the hydrated oxide of copper
precipitated from a solution of a salt of copper by excess of potash
or soda rapidly blackens even though washed with cold water, Péligot
obtains a blue hydrated oxide which resists boiling and heating at 212°
F. He uses any soluble copper salt, but preferably the sulphate. A
very dilute solution of the copper sulphate is treated with ammonia in
excess (aqua ammoniæ or an ammoniacal salt) and precipitated by soda or
potash.

(2) On adding water in excess to a slightly ammoniacal solution of
copper nitrate, the same pigment is obtained.

(3) A mixture of 73 parts silica, 16 oxide of copper, 8 lime, and 3
soda, is fused together at a temperature not much exceeding 800° F. At
higher temperatures there is risk of the pigment turning black.

VERDITER.--This sky-blue and not very durable pigment, used
in water-colour painting, closely resembles Bremen blue (see p. 34) in
composition and manufacture. It consists chiefly of copper carbonate,
mixed with a lesser proportion of hydroxide, sulphate, or oxide,
and occasionally a small quantity of sulphate of lime; and is most
satisfactorily prepared from copper chloride or nitrate, though almost
any salt of copper may be used. The mode of fabrication varies.

(1) To a solution of the nitrate or sulphate is added one of potash
or soda carbonate so long as any precipitate is formed, and this
precipitate, when filtered and washed, is treated with a weak caustic
soda solution.

(2) A hot solution of chloride of lime is added to a hot solution
of sulphate of copper at 62½° Tw. till the precipitate ceases to go
down. The solution of chloride of copper which constitutes the liquor
is filtered off, diluted with water to about 31½° Tw., and treated
with repeated small doses of slaked lime ground exceedingly fine in
water till no more copper is precipitated. The resulting green paste
is drained, filtered, washed, and put into wooden vats; here 8 lb. of
lime paste and 5 pints of potash carbonate solution at 25½° Tw. are
added for every 70 lb. of _dry_ colour contained in the green paste,
the whole mass being thoroughly agitated, then allowed to rest till the
development of the required shade is accomplished, when it is filtered,
washed, and dried.

(3) In some German works the final green paste as prepared in (2) is
put into air-tight vessels, and a solution of 3 lb. ammonium chloride
and 4 lb. sulphate of copper in 7 gal. of water is introduced for each
70 lb. of _dry_ colour in the green paste. After complete admixture of
all the ingredients, the receptacles are fastened up for several days
so that the reactions may proceed out of contact with the air, and
finally the pigment is removed, washed, and dried for use.

=Indigo.=--The well-known blue colouring matter termed indigo is
produced by a great number and variety of plants, distributed
throughout all the tropical countries of the globe. Commercially, it is
obtained chiefly from species of _Indigofera_, as _I. tinctoria_, the
cultivated species of India, furnishing the chief article of commerce,
found also in Madagascar, St. Domingo, &c.; and _I. Anil_, in the
Punjab, W. Indies, and on the Gambia river. Some is also obtained from
_I. argentea_, in Africa and America: _I. Caroliniana_; _I. disperma_,
the cultivated plant of Spain, America, and some of the E. Indies;
_I. cærulea_, the “black indigo” of India; _I. glauca_, in Egypt and
Arabia; _I. pseudo-tinctoria_, cultivated in some parts of the E.
Indies, and said to yield the best dye; _I. cinerea_, _I. erecta_, _I.
hirsuta_, and _I. glabra_, in Guinea. Considerable local supplies are
obtained from the following plants:--_Isatis tinctoria_, in Europe and
China (see Woad); _I. indigotica_, cultivated in some parts of China;
_Amorpha fruticosa_, in Carolina; _Baptisia tinctoria_, wild, in the
United States; _Gymnemia_ (_Asclepias_) _tingens_, in Burmah; _Polygala
tinctoria_, in Arabia; _Polygonum Chinense_, _P. tinctorium_, _P.
perfoliatum_, _P. barbatum_, _P. aviculare_, in China and Japan, and
introduced into Belgium; _Ruellia indigotica_, largely cultivated in
Assam, as well as in India, and at Che-king, in China; _Tephrosia
tinctoria_, and _T. apollinea_, in India and Egypt; _Wrightia
tinctoria_ (_Nerium tinctorium_), the Palas indigo of the Carnatic.

The cultivation of indigo (chiefly _Indigofera tinctoria_) is very
extensively carried on in India, especially in the district included
between 20° and 30° N. lat. The soil best suited for the culture is a
rich loam, with a subsoil which is neither too sandy nor too stiff;
alluvial soils give the best returns, but good crops are sometimes
raised on higher grounds. The land is ploughed in October-November,
after the rains; the seed, about 12 lb. to the acre, is sown in
February-April. Too rapid growth diminishes the yield of dye. In
July-September, the plants are in full blossom, and the harvest takes
place. The preparation of the dyestuff may be performed in either
of two ways, which are distinguished as the “dry-leaf,” and the
“green-leaf” process. The latter is considered the better, and is
the more general; it is conducted as follows:--The flowering plants
are cut down at about 6 in. from the ground, and immediately taken
to the steeping vats, within which they are spread out and pressed
down by beams fitted to the side posts of the tanks. Enough water is
then admitted to cover the plants; if this be delayed, fermentation
may set in and spoil the product. The duration of the steeping is
liable to considerable modification, and needs much judgment and
experience; with a temperature of 96° F. in the shade, 11-12 hours may
suffice; in cooler weather, 15-16 hours may be necessary. Moreover,
very ripe plants require less time than young and unripe ones. The
following general conditions indicate the time for suspending the
maceration:--(1) The sinking of the water in the vat; (2) the immediate
bursting of the bubbles that arise; (3) an orange tint mingled with
the green, when the surface water is disturbed; (4) the emission
of a sweetish, pungent odour, quite distinct from the raw odour of
the unripe liquor. At this point, men enter the vat, and stir up its
contents either by hand or by a wooden paddle. The agitation is at
first gentle, but increases as the fecula begins to separate; this
is known by the disappearance of the froth, and by the colour of the
liquor changing from green to blue. The “beating,” as it is called, is
continued for 1¾-3 hours, the following conditions being a guide as
to its sufficiency:--(1) The ready precipitation of the fecula from a
sample of the liquor, and the madeira-wine colour of the latter; (2)
a brownish colour observed on dipping a cloth into the liquor, and
wringing it out; (3) the appearance of a glassy surface on the liquor,
and the subsidence of the froth with sparkling and effervescence.

Next a little pure cold water, or weak lime-water, is sprinkled over
the surface of the liquor, to hasten the settlement of the fecula,
which occupies 3-4 hours. After this, the water is drained away
from the top, by means of plug-holes in the side of the vat. The
precipitated fecula is then removed to a boiler. Here it is made to
boil as promptly as possible, and is kept boiling for 5-6 hours; it is
constantly stirred, and skimmed with a perforated ladle. After boiling,
it is run off to a straining table, where it stays for 12-15 hours to
drain; next it is pressed for about 12 hours, and then cut, stamped,
and placed to dry. The ordinary dimensions of a steeping-vat are 16 ft.
by 14 ft. by 4½ ft. deep; this will contain about 100 _maunds_ (8200
lb.) of plants, which may yield from 40 lb. downwards of indigo. The
beating-vat is less deep.

Such are the methods of cultivation and manufacture most generally in
use throughout India. In limited districts, however, some modifications
are in vogue. On land subject to inundation, the plants last only one
year. South of the Ganges, the seed is sown at the beginning of the
rains, and the plants remain on the ground for two years, thus giving
a double crop, the second of which is the larger and better. In very
strong land, a third crop is sometimes secured. Occasionally, sesame
is sown on the same ground, and harvested before the indigo is cut.
Small quantities of indigo are grown on poppy lands, and irrigated. The
seed is sown in March-April, and the crop is gathered at the end of
the rains, in time for an opium crop to be taken off the land. Indigo
is sometimes manufactured by collecting the fecula, and dropping it in
cakes to harden in the sun; this is “gaud” indigo, of very inferior
quality. The fecula is improved by boiling it in coppers and pressing
it into boxes. The production of the indigo blue is the result of the
decomposition of the colouring principle of the plant, which exists as
a glucoside. Plants grown on poor soils, and in dry climates, yield
almost the whole of this glucoside to the ordinary process of steeping
and beating described above; but plants raised on rich alluvial soil,
and in damp heat, contain an amount of glucoside which cannot be
utilised by the ordinary process. In order to prevent this waste, which
causes the richest plants to give the least return, it is necessary
either to prolong the fermentation, and raise the heat to 95°-100° F.,
or to add a solution of sugar or glucose to the vat-liquor. Olphert
adopts the use of steam, to raise the temperature of the vat to 111°
F., and thus obtains 25 per cent. more colouring matter.

Japan possesses several large factories for preparing indigo from the
native _Polygonum tinctorium_. The plants, 2-3 ft. high, are cut into
three parts, the uppermost being the most valuable. The best dye is
made from the leaves alone, which, after a few hours’ exposure to air
and sun, are placed in straw bags. They are afterwards removed from
the bags and moistened with water, which must be proportioned with
the greatest exactitude. They are then spread upon, and covered by,
mats, for a few days, after which the sprinkling is repeated. The
process continues for about 80 days, the moistening being renewed
about 25 times for the best leaves, and 9 for the inferior. After
this fermentation, the leaves are pounded in wooden mortars for two
consecutive days, by which they are reduced to a pulp; this is then
formed into balls of dark-blue colour.

The central provinces of Java yield large quantities of indigo, which
are exported to Holland, and thence widely distributed. The indigo
prepared by the natives is of an indifferent quality, in a semi-fluid
state, and contains much quicklime; but that prepared by Europeans
is of a very superior quality. An inferior variety, having smaller
seeds, and being of quicker growth, is usually planted as a second
crop on land where one rice crop has been raised. In these situations,
the plant rises to a height of about 3½ ft. It is then cut, and the
cuttings are repeated three, or even four times, till the ground is
again required for the annual rice crop. But the superior plant, when
cultivated on a naturally rich soil, not impoverished by a previous
heavy crop, attains a height of 5 ft., and grows with the greatest
luxuriance. The plants intended for seed are raised in favourite spots,
on the ridges of rice-fields in the neighbourhood of the villages,
and the seed of one district is frequently exchanged for that of
another. That of the rich mountainous districts, being esteemed of best
quality, is occasionally introduced into the lowlands, and is thought
necessary to prevent that degeneration which would be the consequence
of cultivating for a long time the same plant upon the same soil. The
climate, soil, and state of society of Java seem to offer peculiar
advantages for the extensive cultivation of this plant. The periodical
droughts and inundations of the Bengal provinces are unknown in Java,
where the plant, in favoured situations, may be cultivated nearly
throughout the whole year, and where it would be secure of a prolonged
period of that kind of weather necessary for the cutting. The dye is
prepared in a liquid state by the natives, by infusing the leaves
with a quantity of lime; in this state, it forms by far the principal
dye-stuff of the country. The indigos prepared in Java by Sayers’s
process are of unusually high and constant quality. They contain an
average of 70½ per cent. of indigotine, and a minimum of 65-66 per
cent.; and an average of 2·77 per cent. of ash. Ordinary commercial
indigos seldom attain 65-66 per cent. of indigotine; and their ash
averages about 16½ per cent.

The Philippines produce considerable quantities of indigo, the best
coming from Luzon. The plants suffer from locusts and storms, but the
cultivation is very profitable. The yield of indigotine is large, but
the preparation is conducted in such a primitive manner that the value
of the product is much deteriorated.

In many parts of Africa, as Sierra Leone, Liberia, Abeokuta, the Niger
valley, Natal, Cape Colony, Tunis, and the Soudan, species of indigo
plants are found in a wild state, and from them the natives prepare an
inferior dye-stuff.

In some of the S. States of America, notably S. Carolina, indigo
culture has been attended with more or less success. The method of
preparation pursued here varies but very slightly from the ordinary
Indian process, almost the only important modification being the
addition of a little oil to the liquor in the beating-vat, when the
fermentation becomes too violent. The precipitated fecula is placed
in coarse linen bags, and hung up to drain. The drying is finished by
turning it out of the bags upon a floor of porous timber, and working
it up. It is frequently exposed to the sun for short periods at morning
and evening, and is then placed in boxes or frames, to cure till it is
fit for the market.

Several of the Central American States have figured conspicuously as
indigo producers. The dye is precipitated in the beating-vat by the sap
contained in the bark of Tihuilate (_Yonidium_), Platanillo (_Myrosma
Indica_), or Cuaja tinta. The fecula is left during the night; and,
on the following day, is boiled, filtered, pressed, and sun-dried.
In most districts, the cultivation is declining, partly owing to the
carelessness exhibited in the preparation of the dye.

Indigo is judged commercially by its lightness, by a copper gloss on
the surface, and by exhibiting no foreign ingredients when broken.
There are several ways of testing it chemically, to ascertain
the exact proportion of indigotine present; one method is as
follows:--Finely pulverised indigo, 1 part; green copperas, 2 parts;
and water containing 10 per cent. of caustic soda, 200 parts; are
well boiled in a flask, and left to cool. The clear liquor is exposed
in shallow vessels to the air, when the soluble indigo is oxidised,
and precipitated as pure indigotine. The residue in the flask is thus
treated three times; the whole indigotine is then collected on a
filter, dried, and weighed. The consumption of indigo is still very
large. Artificial indigo has not, as yet, been manufactured on a
commercial scale, nor at a commercial price; but it has been produced,
in the laboratory, from coal-tar derivatives, and further experiment
may reveal a process for preparing the article at a sufficiently low
price to compete with the natural colour.

Several preparations of indigo are in use:--(1) Sulphopurpuric acid,
phenicine, or indigo-purple, is made by mixing 1 part of indigo with 4
parts of sulphuric acid (sp. gr. 1·845), and heating for ½-1 hour; the
acid mass is thrown into 40-50 parts of water, when the purple falls
down; it is collected on a filter, and washed with dilute hydrochloric
acid. (2) Sulphindigotic acid is prepared by mixing indigotine, 1
part, with sulphuric acid (sp. gr. 1·845) 6 parts; the operation must
be performed in a leaden vessel, cooled outside, and the indigo must
be added by degrees, to avoid heating; the mixture is then left for 8
days, when the conversion will be complete. Fuming or anhydrous acid
may be used, in less proportion, but the reaction is more difficult
to manage. Weaker acid will require a longer period, say a month for
“brown acid” (145° Tw.). (3) Sulphindigotic acids are transformed into
neutral paste, or “carmine,” by neutralising with carbonate of soda,
and washing the paste, on a woollen filter, with a solution of chloride
of sodium (common salt).

=Manganese Blue.=--(1) Kuhlmann found a blue mass of manganate of lime
in furnaces used for making calcium chloride by calcining a mixture
of chalk and residues from chlorine making. The formation of this
beautiful coloured manganate he attributes to the decomposition of the
calcium chloride by steam, and to a certain solubility of the lime
in undecomposed calcium chloride. Unsuccessful attempts to reproduce
this result were apparently due to the lime not being under such
favourable conditions for acting upon the manganese oxide as when it
is in solution in the calcium chloride. As accidentally produced in
reverberatory furnaces, the manganate of lime is of an ultramarine
tint, and is insoluble in water though not permanent under its
influence; it is acted upon by the weakest acids.

(2) Bong has proposed several formulæ for making manganese blues,
the ingredients in each case being heated to redness in an oxidising
atmosphere, taking special care to avoid iron. The following are his
recipes:--(_a_) 6 parts soda ash, 5 of calcium carbonate, 3 of silica,
and 3 of manganese oxide; (_b_) 8 of barium nitrate, 2 of kaolin, and
3 of manganese oxide; (_c_) 8 of barium nitrate, 3 of silica, and 3
of manganese oxide. The tint can be varied from violet to green by
altering the proportions.

=Prussian Blue.=--This blue owes its colour to a combination of iron
and ferrocyanogen. The commercial products vary very much in tint,
depth of colour, covering power, and solubility. They are used for a
variety of purposes, nearly all of which require the blue to have some
property different from what it should have for other uses. For some
purposes a green shade blue is wanted, for others a violet shade blue;
some users want the blue to be soluble in water, others for it to be
soluble in oxalic acid, others require it to be insoluble. Ordinary
Prussian blue is insoluble in water, acids, and alkaline salts;
bleaching powder has no action on it, and therefore it is largely used
for tinting paper. It is capable of resisting acids; but alkalies,
such as caustic soda, caustic potash, the carbonates of the same
metals, lime and ammonia, decompose it, oxide of iron and a solution
of a ferrocyanide of the alkali being formed, the decomposition being
shown by a change of colour from blue to a reddish brown. On this
account Prussian blues cannot be used for colouring soaps and alkaline
products, or used as a pigment in distemper painting along with lime.
The change of colour, from blue to brown, by the action of alkalies,
distinguishes this blue from other blues.

Prussian blues require to be tested for their solubility in oxalic
acid, by taking about 20 gr. of the blue, mixing with 1 oz. of water
and 20 gr. of oxalic acid, in which a good blue ought to dissolve
completely. Some brands are soluble in strong hydrochloric acid while
others are not. It is decomposed by boiling sulphuric acid, and turned
green by boiling nitric acid. For all the ordinary uses of a pigment
Prussian blue is quite durable, and possesses a depth of colour and a
definite tint which is proof against the destructive agencies of light
and air; and though its covering powers are not great, it is one of the
most important blue pigments in use.

When a salt of the higher oxide of iron is added to a solution of
yellow prussiate of potash (or ferrocyanide of potassium) a blue
compound is formed which is called Prussian blue. But this is not the
method adopted for its commercial manufacture. In that case a ferrous
salt, the proto-sulphate of iron, is added to a potassium ferrocyanide
solution, the result of which is that a dirty bluish white precipitate
is thrown down. On adding to this a little solution of bichromate of
potash and sulphuric acid, the full deep blue is obtained. This is the
industrial method of manufacturing Prussian blue.

_Yellow Prussiate._--The first step is the preparation of the yellow
prussiate of potash. The manufacture of this substance, although
an industry of considerable importance, is comparatively little
understood, either from a scientific or a practical point of view. At
all events, many prussiate makers seem completely at sea with regard
to the most favourable conditions for carrying on the manufacture, and
there can be no doubt that in many cases great waste occurs, through
ignorance of the various reactions which take place during the process.
The raw materials usually consist of carbonate of potash, iron filings
or turnings, and organic matters containing carbon and nitrogen--such
as dried blood, woollen rags, horn, hair, leather scraps, &c. The
most suitable substances for use are, of course, those containing the
largest proportion of nitrogen. The following are the percentages of
nitrogen in various kinds of animal matter:--

Horn 15 to 17
Dried blood 15 to 17
Woollen rags 10 to 16
Sheep shearings 16 to 17
Calves’ hair 15 to 17
Bristles 9 to 10
Feathers 16 to 17
Hide clippings 4 to 5
Old shoes 6 to 7
Horn charcoal 2 to 7
Rag charcoal 2 to 12

Animal matters always contain more carbon than is necessary for the
formation of cyanogen by combining with the nitrogen also present.
Consequently, when such substances are heated with pearlash, the
excess of carbon reduces a portion of the carbonate to the metallic
state, and this potassium combines with the cyanogen to produce
potassium cyanide. The manufacture of yellow prussiate of potash may
be conveniently divided into three stages: (1) The production of the
molten mass technically known as “metal”; (2) the lixiviation; and (3)
the crystallisation.

(1) The “metal” is made by fusing animal matters with pearlash, almost
invariably with the addition of iron scrap. The animal substances are
sometimes used in their original condition, whilst sometimes they are
previously charred. Generally speaking, however, a judicious mixture
of the fresh and charred materials has been found to give the best
results. The charcoal which is left on carbonising animal matters
contains a certain amount of nitrogen, decreasing in proportion as the
temperature rises; but a smaller quantity of charcoal is also thereby
produced. For example: 100 parts of rags carbonised at a certain
temperature left 75 parts charcoal containing 12 per cent. of nitrogen,
while the same rag carbonised at a higher temperature yielded 25 parts
of charcoal, which contained only 2 per cent. of nitrogen. The animal
matters employed should not leave much ash on ignition, as this would
both thicken the mass and decompose a portion of the potash. In this
respect sand is specially objectionable, for on ignition 1 part will
decompose 2 of pearlash, owing to formation of silicate of potash. It
is not necessary that the pearlash should be quite pure; in fact, a
certain proportion of sulphate is stated to be useful, as it is changed
into sulphide by ignition with the carbonaceous materials.

The theory of the formation of yellow prussiate of potash may be
briefly stated as follows: The carbonate and sulphate of potash
react with the carbon, nitrogen, and iron, forming in the first
instance sulphide of potassium, which afterwards converts the iron
into sulphide, whilst potassium cyanide is simultaneously produced.
It should be here explained that ferrocyanide of potassium (yellow
prussiate) is not formed during the ignition of the above mentioned
materials, but results from the lixiviation of the fused mass with
water, when the cyanide of potassium and iron sulphide decompose
each other, producing ferrocyanide and sulphide of potassium. It is
quite obvious that even if any ferrocyanide were produced during the
process of fusion, it would almost immediately be decomposed, at the
intense heat to which the mass is subjected, into potassium cyanide,
iron carbide, and nitrogen gas. If any doubt were felt on this point,
the experiments of Liebig conclusively prove that the formation of
ferrocyanide takes place on dissolving the ignited mass in water, but
not previously. Liebig found that if the fused mixture be allowed
to cool, and then treated with moderately strong alcohol, potassium
cyanide alone is extracted, and the residue when dissolved in water
no longer yields ferrocyanide. As ferrocyanide is not formed during
the process of fusion, the presence of iron in the preliminary stages
may appear superfluous; but such is not the case. The presence of iron
is necessary for two reasons, firstly, because the sulphate of potash
which is generally present is converted into sulphide and bisulphide,
and these, in the absence of iron, would decompose some of the cyanide
of potash into sulphocyanate, thereby causing a loss of cyanogen so
far as yellow prussiate is concerned; and secondly, because potassium
bisulphide has a very corrosive action on the iron pot in which the
fusion takes place. When iron is present it readily decomposes any
alkaline sulphides, thereby preventing formation of sulphocyanate, and
being itself converted into iron sulphide, which is again changed into
prussiate by the action of the aqueous cyanide.

Pear-shaped iron pots were formerly used for fusing the raw materials.
The arrangement now generally adopted in large English works consists
of a series of iron pots almost hemispherical in shape, set in
brickwork, and each heated by a separate fire and circular flue. These
vessels are closed by iron lids, with apertures for the admittance of
animal matters, the aperture being at once closed by a slide after each
addition. Through every lid there passes a vertical spindle, carrying a
set of blades for mixing the materials, and set in motion by a suitable
shaft worked by steam power. Instead of the ordinary iron pots,
reverberatory furnaces are often employed, especially in Germany. The
reason for this preference is, that ordinary iron vessels are worn out
in a comparatively short time, the destructive action being greatest on
the under surface of the muffle. A much larger quantity of raw material
can also be operated upon at one time if a reverberatory furnace be
used. The mode of procedure depends to some extent upon the condition
of the organic materials employed. If fresh, the muffle or furnace must
be left open, so as to permit the mixture to be well and frequently
stirred, and additions to be made at intervals until eventually
ammonia ceases to be evolved. The furnaces are arranged in such a
manner that when the carbonate of potash has once become fused the
doors of the fire-place may be shut, and no fresh firing is required
during the introduction of the animal matters. The molten mass is kept
well stirred by means of a thick iron bar, suspended by a chain, and
fixed in an aperture in the side of the furnace. By the use of this
arrangement the stirring is much more easily and thoroughly effected
than is the case with the old fashioned pots. Ordinary reverberatory
furnaces cannot be used for the fusion, because the silica in the
hearth would combine with the potash to form silicate of potash.
Gas generators with air blast are now sometimes employed instead of
ordinary fuel in the manufacture of yellow prussiate of potash. Several
advantages are gained by operating in this manner, especially that of
permitting the regulation of temperature and the admission of oxygen,
so as to obtain an ordinary, a neutral, or a reducing flame, according
to requirements. In the preparation of the “metal,” for every 100
parts of pearlash from 100 to 125 parts of fresh animal substances are
required, together with 6 or 8 parts of iron in some form or other. The
pearlash, or a mixture of 1 part of pearlash with 2 to 4 parts “blue
salt” or “blue potash” (this substance will be referred to later on),
is melted in the furnace and heated to bright redness, so that the
temperature of the mass may not be reduced too much by the addition
of the animal matters. These, in their original condition, or an
equivalent quantity of carbonised materials, together with the proper
proportion of iron, are then introduced--first pretty frequently,
afterwards at longer intervals. Each addition of animal matter causes a
somewhat violent frothing and escape of combustible gases, along with
water and carbonic acid, and the whole becomes thick--not so much owing
to the introduction of solid substances as by the fall of temperature,
resulting from the production of such large quantities of gas. In
order to hasten the decomposition, vigorous stirring must be applied.
When the reaction is at an end, the semi-fluid mass is transferred to
cast-iron dishes, and the furnace is again filled with carbonate of
potash and heated. In this way four or five charges may be accomplished
every day, and the process carried on continuously. The most favourable
conditions for effecting the melting part of the process are attained
when the heat approaches whiteness, and a bright, clear flame is
produced as soon as the raw materials are introduced. According to one
authority, woollen rags and good pearlash, with a small proportion
of waste iron, have produced the largest yield of yellow prussiate,
although even in this case two-thirds of the total nitrogen present was
lost in the form of ammonia.

(2) Lixiviation.--The fused mass, if properly prepared, should yield
about 16 per cent. of prussiate on dissolving in water. In this part
of the process, the “metal” when cold is broken into lumps and placed
in cold water mixed with the weak lyes from former operations. Heat
is then applied until the temperature rises to about 180°-190° F.,
and the liquid is stirred vigorously so as to promote rapid solution,
because some of the potassium cyanide is apt to be decomposed during
lixiviation. When the solution attains a density of 30°-40° Tw. it
is left to clarify, the heat being withdrawn. The clear solution is
decanted, and evaporated in pans, which are generally heated by the
waste heat of the furnaces. When it has a density of 54° Tw. it is run
off into the crystallisers, where it deposits the crude salt.

(3) Crystallisation.--This is a very important stage of the
manufacture, as it is the final process by which the crude prussiate
is rendered sufficiently pure to be placed on the market. The impure
substance is dissolved in warm water until the solution stands at 54°
Tw.; after all insoluble matter has deposited, the clear liquor is
placed in the crystallising vessels. These are occasionally made of
wood; but when such vessels are used, the crystallised salt generally
possesses a green colour, which is believed to be due to the tannin
present in the wood. On this account cast-iron crystallisers are more
frequently employed. The crystallisation proceeds slowly--often going
on for several weeks in large vessels. The mother liquor is then drawn
off, and if not too impure is used for dissolving fresh quantities
of the crude prussiate. The ferrocyanide is deposited in crusts in
the crystallisers; but by hanging lumps of the solid salt in the
solution, long clusters of crystals may be obtained, and by suspending
these in fresh prussiate lyes immense crystals are produced. From 100
parts crude prussiate about 90 parts pure potassium ferrocyanide are
obtained, or sometimes in the case of purer materials 97 parts.

Sulphate of potash is often present in commercial yellow prussiate.
The separation of this impurity is best effected on the large scale by
evaporating the prussiate solution to a density of 62° Tw., at which
point most of the sulphate will crystallise out. If the clear liquor be
then drawn off, diluted to 52° Tw., and allowed to cool, almost pure
potassium ferrocyanide will gradually deposit. This may be rendered
absolutely pure by gently fusing the crystals, dissolving in water, and
treating with a small quantity of acetic acid, which will decompose
any carbonates and cyanides. On adding sufficient strong alcohol, the
ferrocyanide is precipitated, and when crystallised once or twice more
from water it may be regarded as chemically pure.

Blue salt.--This substance, to which we have previously referred, is a
residue obtained in the manufacture of prussiate of potash. The last
mother-liquor contains a large quantity of carbonate of potash, along
with smaller amounts of hydrate, silicate, chloride, and sulphocyanate.
It is concentrated until the liquid has a density of 90° Tw., when most
of the chloride, silicate, &c., separates out, and the strong liquor
containing the greater proportion of the carbonate is evaporated to
dryness, and calcined in a reverberatory furnace. The dry residue
constitutes the “blue salt” or “blue potash,” and contains from 70
to 80 per cent. carbonate of potash. It may be employed instead of
pearlash, or mixed with it, for the next batch of yellow prussiate. The
composition and amount of the insoluble residue left on lixiviation of
the “metal” vary according to the proportions and character of the raw
materials used. Other conditions being equal, horn gives the lowest
percentage of insoluble matter on lixiviation.

The large proportions of potash and phosphates contained in the
insoluble residues render them well suited for use in the manufacture
of artificial manures. As already mentioned, when regarded from a
scientific or economical point of view, the yellow prussiate industry
is carried on under very imperfect conditions. In addition to the
amount of potash, there is a very considerable waste of nitrogen,
firstly, because the larger proportion of that element present in the
animal substances is not converted into cyanogen at all, but passes
off chiefly in the form of ammonia salts; and, secondly, because
part of the potassium cyanide which is actually produced is lost by
decomposition, and another portion is left in the mother liquor. It
has been calculated that out of every 100 parts of ferrocyanide which
should theoretically be obtained, 4 parts are lost when fairly pure
materials have been employed, and 14 in the case of impure ingredients.

The following analyses indicate the percentage composition of two
samples of insoluble residue:--

No. 1. No. 2.

Sulphate of potash, &c. 9·06 3·21
Phosphates of lime, magnesia and iron 13·74 6·24
Oxide of iron 13·34 19·58
Lime and magnesia 5·08 7·23
Sand and silica 23·97 29·24
Charcoal and moisture 34·81 34·50
------ ------
100·00 100·00

According to Karmrodt, the following proportions of the nitrogen
contained in various animal substances are actually converted into
cyanogen during the manufacture of yellow prussiate of potash:--

Per cent.

Woollen rags 16
Horn 20
Leather cuttings 33
Cow hair 14
Dried blood 16
Horn charcoal 56
Rag charcoal 33

As is well known, human excreta contain a considerable proportion of
nitrogen, and there seems no reason why this should not be employed
in the manufacture of yellow prussiate. It is quite possible that
municipal bodies might find this a convenient and profitable plan
of disposing of a portion of the sewage with which they have to
deal. It is obvious to all persons who have given this subject much
consideration, that the nitrogen required in the manufacture of yellow
prussiate of potash might be obtained with comparative ease from the
surrounding atmosphere. Indeed, from a theoretical point of view this
seems a charming process. About fifty years ago the Society of Arts
awarded Lewis Thompson a medal in connection with this very process.
Thompson ignited a mixture of 2 parts pearlash, 2 parts coke, and 1
part iron turnings in an open crucible for a considerable time at a
full red heat. The resulting black mass was found to contain a large
quantity of ferrocyanide, together with excess of carbonate of potash,
&c. This process, or a similar one, in which a current of air was
passed over a mixture of charcoal and iron saturated with carbonate of
potash, was tried on a large scale for two years at Bramwell’s works
at Newcastle. About 1 ton of yellow prussiate was made daily by this
process; but it was not found to work profitably, and was eventually
abandoned, chiefly, it is said, owing to the large amount of fuel
required, and because the cylinders, whether of iron or fireclay, were
not able to stand for any length of time the intense heat to which they
were subjected.

The annexed illustrations, Figs. 14 to 17, show the arrangement of a
prussiate of potash furnace at Sir E. Buckley’s works, at Clayton,
Manchester, which are well designed to prevent nuisance: A, iron pot;
B, fire-place; _a_, cover of pot; _b_, stirrer; _c_, hinged pipe
conveying vapours to the flues; _d_, flues surrounding the pot, and
leading to the chimney-shaft; _e_, chain to lift up cast-iron vapour
hood.

Brunquell, a German manufacturer, has criticised the present method
of conducting operations, and proposes that it is necessary as far
as practicable to aid the secondary formation of cyanogen by ammonia
and incandescent charcoal, and to avoid loss of potash by using pure
animal substances, and preventing contact with the solid products of
combustion from the furnace. With this view he adopts a horizontal
reverberatory furnace, the hearth of which is a cast-iron tray about
4½ ft. long, 4 ft. wide, and 3½ in. deep. The crown of the furnace is
built as flat as possible, the working space is limited, and the charge
is kept from contamination by the fire. Such a furnace, despite certain
drawbacks, presents important advantages. Fuel is economised; the
process is hastened so that seven or eight charges can be dealt with
in a day, instead of only four; and the furnaces cost less and endure
longer. The charge consists of 220 lb. potash, of which two-thirds is
from evaporated mother-liquors, and one-third fresh; 44 lb. animal
charcoal from the carbonisation of substances poor in nitrogen; 140-150
lb. of pure animal matters as dry as practicable; and 17½ lb. iron. The
firing is urged and the charge is stirred till all the potash is fused,
when the ash-pit is closed, and the damper turned on for charging half
the animal charcoal. The firing and stirring are again pushed on till
the proper consistency is attained, and potassium vapour begins to burn
off. In this state the mass is ready to receive the animal

[Illustration: Figs. 14, 15, 16, 17.--YELLOW PRUSSIATE
FURNACE.]

substances, those rich in nitrogen being first added in small portions
at a time. Their effect is to render the mass hard, dry, and difficult
of fusion, whereupon the remainder of the animal charcoal should be
promptly introduced. After thorough agitation, the working door is
closed for a short time, and the contents of the furnace are rapidly
discharged into a covered iron pan.

The character of the animal matters employed varies so much that it is
impossible to lay down hard and fast rules for the proportions of the
several ingredients, or the duration of the roasting. Nor is the value
of a raw material always in proportion to its richness in nitrogen,
because the poorer material may waste less potash, consume less fuel,
and require less labour. The addition of iron filings or turnings is
useful only in prolonging the life of the cast-iron crucibles.

_Combination of the Cyanide and Iron Solutions._--A great number of
recipes are in vogue for combining the two solutions of ferrocyanide
and an iron salt, both with reference to their proportions, and to the
addition of foreign matters of various kinds. These variations in the
formulæ give rise to distinct names for some kinds of Prussian blue,
which will be referred to below. The ordinary common Prussian blue has
a greenish tendency, and is chiefly made according to one or the other
of the following directions:--

(1) Mix a solution of 100 lb. yellow prussiate with a solution of 100
lb. green copperas (ferrous sulphate) and 18 lb. alum, to which 9 lb.
sulphuric acid has been added, and let the mixture stand for 2-3 hours,
or until the solid portion has completely settled out. Decant the clear
supernatant liquor, and well wash the precipitate with clean waters.
Finally throw it on a filter and subject it to repeated disturbance,
so as to ensure the admission of air to every particle, in order that
the requisite oxidation may take place. The proportion of alum used
is subject to very great variation according to individual fancy; it
renders the subsequent grinding of the pigment a very much easier
matter, but it causes the shade of blue to be paler than it otherwise
would be.

(2) The simple solutions of green copperas and yellow prussiate in
equal proportions are mixed together without any other ingredient being
added, and the precipitate produced is washed, filtered, and aërated as
in (1). It is, however, inferior by reason of the oxide of iron formed
in the pigment spoiling the purity of the colour, and necessitating the
treatment of the wet mass with hydrochloric acid, at some expense, for
removal of the iron oxide.

ANTWERP BLUE.--This pale variety of Prussian blue has but
little importance now. It is prepared by adding a solution of 4 lb.
yellow prussiate in 5-6 gallons of water to one of 2 lb. sulphate
of iron, and 1 lb. each of alum and sulphate of zinc in an equal
quantity of water. The resulting pigment consists of a mixture of the
ferrocyanides of iron, alumina, and zinc; it is washed, filtered,
aërated, and dried as other forms of Prussian blue.

BONG’S BLUE.--When cyanide of potassium is added to an
acid solution of a copper salt, a red colour is produced, which has
already been mentioned by different observers. The substance formed
is very changeable, at least in the liquid where it is formed. It
is decomposed by acids, alkalies, cyanide of potassium, and even
decomposes spontaneously, the colour changing to yellow. It is
precipitated by insoluble cyanides; hence when a dilute acid is added
to the red solution, the dye is at once thrown down along with the
cyanide of copper. If the precipitate thus obtained is treated with
sulphuretted hydrogen, it is decomposed and the substance is set free.
This substance can combine with iron, like cyanogen, so as to conceal
the properties of the iron. This compound is very permanent, and has
lately been studied by Bong, who gives the following directions for its
preparation:--

Cyanide of potassium is added in excess to an acid solution of a
copper salt until the red colour at first formed has disappeared,
when a ferric salt is at once added. On the addition of the iron salt,
of course, a copious precipitation of Prussian blue takes place,
and the liquid again turns to a dark purple-red. To separate the
colouring substance from the alkaline salts in the liquid, a dilute
acid is added, which precipitates it and the cyanide of copper. This
precipitate is combined with the Prussian blue, which also contains
a considerable quantity of the colouring substance, and then treated
with a boiling solution of carbonate of ammonia, in which it dissolves.
As the cyanide of copper also goes into solution, it is separated by
again precipitating it with an acid, and treating the precipitate with
sulphuretted hydrogen. The colouring substance thus liberated now
contains a certain amount of hydroferrocyanic acid, which is removed
after neutralisation by acetate of lead. It is now filtered, and the
purification is completed by precipitating with a silver salt and
treating the precipitate with sulphuretted hydrogen.

This purple-coloured compound crystallises very indistinctly. To
determine its composition, Bong precipitated it with acetate of copper.
When dried at 212° F., the rose-coloured precipitate had the following
composition: Carbon 24·31, nitrogen 28·04, hydrogen 1·88, iron 13·66,
copper 17·67, oxygen 14·44. Total 100·00. These numbers correspond to
the formula Cu, Fe Cy_{4} (HO)_{4}.

This substance is likewise precipitated by salts of zinc, mercury, and
silver. All these precipitates are pink or purple, very beautiful, and
of remarkable brilliancy. They are soluble in alkalies. Iron salts
yield no precipitate, nor do lead salts, except in the presence of
ammonia, when a blue-violet precipitate is formed. When treated with
sulphuretted hydrogen, these precipitates yield purple-red and acid
liquids, which undergo change in the air, especially if warm, forming
Prussian blue. When these liquids are neutralised with alkali, purple
compounds are formed, which are permanent in the air, soluble in water,
slightly so in alcohol, and insoluble in ether. Their colouring power
is exceptionally great. These pigments will unite with ferrocyanides,
and in its preparation such a compound is produced in considerable
quantity; it is likewise of a purple colour, and gives a rose-coloured
precipitate with acetate of lead. Both alone and in this compound it is
very permanent; it resists the action of sulphurous acid, concentrated
and boiling alkalies, and dilute acids, but is rapidly destroyed by
chlorine and nitric acid. If this pigment could be prepared cheaply
enough, it would probably be used with advantage in the arts, on
account of its resistance to chemical reagents and light, the variety
of its shades, and its brilliancy. It does not colour fibres directly,
but can readily be fixed on them from slightly acid solutions, if they
are previously mordanted with metallic oxides.

BRUNSWICK BLUE.--This pigment is made in pale, medium, and
deep shades, and is an extremely useful colour, being very fine,
requiring no grinding, thoroughly permanent in light and air, hardly
acted upon by acids, but turned brown by alkalies, and liable on
standing to separate into two portions--a white and a blue--the latter
coming to the surface while the former sinks, and necessitating a
thorough stirring of the paint before use.

It generally consists simply of barytes, or gypsum, or china clay,
coloured by a small percentage of Prussian blue, with or without the
addition of a lesser proportion of ultramarine. The barytes or other
base is very thoroughly agitated in water, while a solution of green
copperas and a solution of yellow prussiate are gradually added without
ceasing the agitation. When the incorporation of the ingredients has
been completely accomplished, the precipitate is settled, washed,
filtered, and dried. Following are a few recipes:--

Pale. (1) 1 cwt. barytes, 1 lb. green copperas, 1 lb. yellow
prussiate.

Pale. (2) 1 cwt. china clay, 2 lb. green copperas, 2 lb. yellow
prussiate.

Pale. (3) 1 cwt. gypsum, 1½ lb. green copperas, 1½ lb. yellow
prussiate.

Medium. (1) 1 cwt. barytes, 3 lb. green copperas, 3 lb. yellow
prussiate.

Medium. (2) 1 cwt. china clay, 6 lb. green copperas, 6 lb. yellow
prussiate.

Medium. (3) 1 cwt. gypsum, 4½ lb. green copperas, 4½ lb. yellow
prussiate.

Deep. (1) 1 cwt. barytes, 5 lb. green copperas, 5 lb. yellow
prussiate.

Deep. (2) 1 cwt. china clay, 10 lb. green copperas, 10 lb. yellow
prussiate.

Deep. (3) 1 cwt. gypsum, 7½ lb. green copperas, 7½ lb. yellow
prussiate.

In each case about 50-60 gallons of water are required.

To determine the amount of barytes present in a sample, boil about 50
gr. with caustic soda, filter, wash the residue free from soda, treat
with sulphuric acid, well wash the insoluble residue, dry, and weigh.

CHINESE BLUE.--This well-known and favourite form of Prussian
blue is prepared with great care, and is usually sold in fine powder
or little cubes. Its composition is virtually identical with that
of ordinary Prussian blue, but it is more free from impurities, and
shows a fine bronze bloom or lustre on newly fractured surfaces. Being
pure, it is entirely dissolved by oxalic acid; and its composition
is about 52 per cent. oxide of iron, 43½ cyanogen, and 4½ water. In
dyeing and calico-printing it is extensively employed. Its tint varies
from greenish to violet, according to modifications in the method of
manufacture, the chief difference being that yellow prussiate gives a
greenish tone and red prussiate a violet.

The process of preparation is mainly as follows. In about 40 gallons
of cold water dissolve 1 cwt. of green copperas selecting it carefully
for freedom from insoluble oxide; add about 5 pints of sulphuric acid.
This liquor very rapidly undergoes oxidation, by which oxide of iron
is thrown down, and the solution is rendered unfit for making the best
quality pigment. Therefore it should be prepared only immediately
before it is used. In another vessel containing about 40 gallons of
cold water, dissolve 1 cwt. of yellow prussiate (if a green shade is
desired), or of red prussiate (if a violet tint is wished for). Even
larger quantities of water may be used for the solutions, as the more
dilute they are the finer is the colour precipitated and the greater
the lustre on the surface of the finished pigment.

When the two solutions of yellow or red prussiate and acidified green
copperas are brought together, a bluish-white precipitate is thrown
down. This is allowed to completely separate itself, and then the clear
supernatant liquid is drawn off.

The next step is to thoroughly oxidise the precipitate. This cannot be
satisfactorily accomplished by utilising the oxygen of the atmosphere,
as is done in other cases, because that method entails the production
of a certain amount of oxide of iron, which prejudicially affects the
purity of colour of the finished article. Of the chemical oxidising
agents which are available, the most satisfactory in point of cost
and efficiency is chloride of lime (bleaching powder). For each cwt.
of green copperas, mix about 20 lb. of bleaching powder into a thin
cream with water, and add it, in small quantities at a time, to the
precipitate, constantly stirring so as to ensure the absorption of
the whole of the chlorine by the blue. Without the addition be made
gradually and under agitation, the chlorine will be generated more
quickly than it can be absorbed, entailing a waste of gas and a noxious
vapour to be breathed by the workmen. Sometimes the bleaching powder is
added at an earlier stage, viz. to the green copperas solution, and in
that case the blue assumes a violet tone.

After the addition of the bleaching powder solution to the bluish-white
precipitate, it is acidified with hydrochloric acid, which develops
the blue. When the whole has settled, the supernatant liquor is drawn
off, and the blue powder is well washed and strained on a filter,
then placed in pans and dried very gradually indeed in the dark, at a
temperature never exceeding 130° F. The slower the drying the better
is the gloss of the pigment. It is most essential that iron be excluded
during the final grinding operation, or it may cause ignition of the
mass, and its conversion into oxide of iron would speedily follow.

It has been proposed to treat the white precipitate (obtained in the
usual manner from green copperas and yellow prussiate) by the chlorine
contained in aqua regia (nitro-hydrochloric acid). The copperas,
however, must be as free as possible from basic sulphate (oxide), which
is ensured by keeping a little metallic iron in the acid solution
of copperas. It is also desirable to effect the precipitation with
crude prussiate, so as to avoid absorption of oxygen and premature
development of the blue colour. Habich considers that the mistake is
generally made of using too little copperas, and he has found that when
90 lb. of copperas have been added to 100 lb. of yellow prussiate, a
drop of iron solution in the filtered liquor produces no precipitate,
while the white precipitate has carried with it a certain proportion of
prussiate, which can be washed out. He therefore proposes to avoid this
waste by pouring the copperas solution into the prussiate solution,
with constant agitation, till no further precipitate goes down, then
adding one volume of the copperas solution equal to one-ninth of that
already used. After fifteen minutes stirring, it is certain that all
the prussiate carried down is decomposed.

The drained precipitate is blued (peroxidised) by adding aqua regia
prepared several days previously, and in proportions depending on the
strengths of the two acids. Generally, the aqua regia mixture will be
100 lb. of commercial nitric acid at 30° B. (containing 35·4 lb. of
anhydrous acid) and 62·2 lb. commercial hydrochloric acid at 23° B.
(containing 23·9 lb. of the anhydrous acid); and 40 lb. of this mixture
will suffice for bluing the precipitate resulting from 100 lb. yellow
prussiate. The addition of the aqua regia should take place in a
wooden vessel with constant agitation.

According to another modification, the white precipitate obtained in
the usual way is blued by adding a solution of perchloride of iron,
which may be made from a hematite ore free from clay and carbonate of
lime, or from rouge. The iron oxide, from whatever source, is ground
to a very fine state, and treated with crude hydrochloric acid in
a lead-lined tank, where the mixture remains for several days, and
is constantly stirred. When saturated with iron the clear liquid is
withdrawn for use. To receive it, the white precipitate is rapidly
heated to boiling in a copper vessel, and is then transferred to a
wooden vat, and the iron perchloride solution is stirred in till the
desired tint is produced. The pigment is washed and dried in the
ordinary way, while the supernatant liquor (essentially protochloride
of iron) is poured over old scrap iron and used instead of copperas for
a fresh batch of yellow prussiate.

A solution of perchloride of manganese may be used instead of
perchloride of iron. Inferior qualities of manganese ore can be
employed, and the residues left after treatment with hydrochloric acid
may be washed and dried for sale as purified or peroxidised manganese.

PARIS BLUE.--(1) A synonym for the violet-tinted kind of
Prussian blue.

(2) A series of compounds described below. [_a_] A thorough mixture of
2 parts sulphur and 1 part dry carbonate of soda is gradually heated
in a covered crucible to redness or till fused; a mixture of silicate
of soda and aluminate of soda is then sprinkled in, and the heat is
continued for an hour; the little free sulphur present may be washed
out by water. [_b_] An intimate mixture of 37 parts china-clay, 15
parts sulphate of soda, 22 parts carbonate of soda, 18 parts sulphur,
and 8 parts charcoal, is heated in large crucibles for 24-30 hours;
the mass is re-heated in cast-iron boxes at a moderate temperature
till the desired tint appears, and is finally pulverised, washed, and
dried. [_c_] Gently fuse 1075 oz. crystallised carbonate of soda in its
water of crystallisation; shake in 5 oz. finely-pulverised orpiment,
and, when partly decomposed, as much gelatinous alumina hydrate as
contains 7 oz. anhydrous alumina; add 100 oz. finely-sifted clay, and
221 oz. flowers of sulphur; place the whole in a covered crucible,
and heat gently till the water is driven off, then to redness, so
that the ingredients sinter together without fusing; the mass is then
cooled, finely pulverised, suspended in river-water, and filtered. The
product is heated in a covered dish to dull redness for 1-2 hours, with
occasional stirring. Colourless or brownish patches may occur, and must
be removed.

SAXON BLUE.--Following is a recipe for the preparation of this
pigment, which possesses limited importance.

Dissolve 8 lb. alum and 1 lb. green copperas in 16 gallons of
water. Add separate solutions of pearlash and yellow prussiate till
precipitate ceases to go down. Collect the precipitate when it has
completely settled; wash thoroughly, and dry.

SOLUBLE BLUE.--This term is applied to a variety of Prussian
blue which, while possessing no difference in the matter of chemical
composition, yet has the distinctive feature of being soluble in water,
which the other varieties are not. It no longer enjoys the popularity
it once had as a dye, on account of the severe competition of the
coal-tar colours. Below are some of the most satisfactory formulæ for
its preparation.

(1) Mix 10 lb. of Prussian blue thoroughly in about 10 gallons of cold
water. Then add 5 lb. of yellow prussiate and let the whole mass boil
steadily for several hours. Strain off the liquor and well wash the
precipitate on a filter. Finally dry for use.

(2) Dissolve about 1 cwt. of red prussiate in water and make the
solution hot. Prepare another solution of about 73 lb. of green
copperas in hot water. Mix the two solutions together and boil them for
about a couple of hours. Allow the solid matters to settle out, then
put them on a filter and wash with clean water until a blue coloration
manifests itself in the drainings. The blue residue is then dried as
usual.

(3) Make one solution of 10 lb. of yellow prussiate, and another of 8
lb. of green copperas, water being the solvent in both cases. Mix these
two solutions together and give them an hour’s boiling.

Add 3 lb. of a mixture of nitro-sulphuric acid, containing 2 parts of
the former to 1 of the latter. Boil for another hour. Let the solid
pigment precipitate itself thoroughly, and then filter, wash, and dry
as in the other cases.

(4) Dissolve about 1 cwt. of perchloride of iron and 10 lb. of sulphate
of soda in water. Also dissolve in another vessel 2 cwt. of yellow
prussiate and 10 lb. of sulphate of soda. Pour the first solution
into the second (never the contrary) and take care that the prussiate
solution is always preponderant. The Glauber’s salt is useful in
rendering the precipitation of the blue pigment more complete by
reason of the insolubility of the latter in saline fluids. When the
blue sediment is all thrown down it is drained off on a filter, and
repeatedly washed till a blue tint appears in the wash-waters, when it
is dried for use.

TURNBULL’S BLUE.--This is an old-fashioned name often applied,
like the term Paris blue, to the violet shades of Prussian blue which
have been prepared with red prussiate.

=Ultramarine.=--According to Rowland Williams, F.C.S., natural
ultramarine is, perhaps, the most beautiful blue pigment known. It
was formerly, and is now to a small extent, manufactured (chiefly
for artists’ use) from lapis lazuli, a blue mineral which occurs,
intermixed with limestone and iron pyrites, in Siberia, Thibet, and
China. In order to obtain ultramarine from lapis lazuli, the roughly
pulverised mineral is ignited, dipped into vinegar to remove carbonate
of lime, and then reduced to the finest possible state of division.
The powder is next mixed with a cement composed of rosin, linseed oil,
white wax, and Burgundy pitch, and the resultant paste is worked under
water until all the ultramarine is separated. The ultramarine is washed
several times with water, and afterwards with alcohol, which removes
any of the resinous compound which may have adhered. When treated in
this manner, lapis lazuli yields from 2 to 3 per cent. of ultramarine.
According to Clement and Desormes, lapis lazuli has the following
composition:--

Per cent.

Soda 23·2
Alumina 34·8
Silica 35·8
Sulphur 3·1
Carbonate of lime 3·1
-----
100·0

It will be seen, therefore, that ultramarine essentially consists of
alumina, silica, soda, and sulphur, and may be regarded as a sodium
aluminium sulphate, in combination either with polysulphide of sodium
alone, or with a polysulphide and a polythionate of sodium. Clement
and Desormes believe that the iron in lazulite (lapis lazuli) is an
accidental impurity, and is neither essential to the mineral itself nor
to the ultramarine derived from it. There is still some doubt on this
point, however, many eminent chemists holding the opinion that iron is
a necessary constituent of ultramarine blue.

Natural ultramarine has been almost entirely replaced by the artificial
product, since methods have been devised for the manufacture of the
latter on a large scale. The possibility of preparing artificial
ultramarine suggested itself in a curious manner. About seventy years
ago a French alkali maker noticed the occasional appearance of a blue
coloured substance in his soda furnace. On analysis, Vauquelin found
the substance to have the same chemical composition as lapis lazuli,
and this incident led him to believe that ultramarine might be built up
from its elements. Several years passed away before Guimet succeeded in
manufacturing artificial ultramarine on anything like a large scale,
but Gmelin is said to have prepared it in small quantity half a dozen
years previously. There are four varieties of artificial ultramarine:
(1) the pure deep blue, equal in colour to average native ultramarine;
(2) pale blue; (3) violet or pink ultramarine; (4) green ultramarine.
The latter is obtained in the first stage of the ultramarine
manufacture, being the result of incomplete ignition of the materials
employed. Ultramarine is generally manufactured by one of the following
processes:--(_a_) “Sulphate”; (_b_) “Soda”; (_c_) “Silica.”

(_a_) “_Sulphate_” _Ultramarine_.--This may be prepared from sulphate
of soda (Glauber’s salt), charcoal, and kaolin (china clay). The
materials should be as free as possible from iron, and it has
been found that clay having approximately the formula Al_{2}O_{2}
(SiO_{2})_{2} gives the best results. The clay and sulphate of soda
must be thoroughly calcined. They are then intimately mixed with
charcoal in the following proportions:--

Per cent.

Clay 48·3
Sulphate of soda 43·5
Charcoal 8·2
-----
100·0

Sometimes a portion of the sulphate of soda is omitted, and some
carbonate of soda and sulphur added instead. The composition of the
mixture then becomes:--

Per cent.

Clay 47·2
Sulphate of soda 19·3
Carbonate of soda 19·3
Charcoal 8·1
Sulphur 6·1
-----
100·0

Caustic soda is also sometimes used instead of carbonate. These
mixtures (whether sulphate alone or sulphate and carbonate) are made
with a view to have the soda present in sufficient amount to combine
with one-half the silica contained in the clay, and to leave sufficient
soda to form polysulphide of sodium with a portion of the sulphur.
There should then remain enough soda and sulphur to produce ordinary
sulphide of sodium (Na_{2}S). If either of the two mixtures be ignited
out of contact with air, a white compound is formed, which is sometimes
termed white ultramarine. On leaving this exposed to the atmosphere for
some time it becomes green, and on further ignition, with free access
of air, it is converted into ultramarine blue. In actual working the
carefully prepared mixture of the above mentioned materials is heated
for several hours to a high temperature in fire-clay crucibles, only a
limited supply of air being allowed to enter, and the temperature being
eventually raised to a white heat. The product of this operation, when
cool, has a grey or yellowish-green appearance. It is washed several
times with water, dried, reduced to a fine powder, and then represents
the green ultramarine of commerce. Stölzel found that green ultramarine
had the following composition:--

Per cent.

Alumina 30·11
Silica 37·46
Sodium 19·09
Sulphur 6·08
Iron ·49
Calcium ·45
Chlorine ·37
Oxygen 5·19
Sulphuric acid ·76
Magnesia, potash, and phosphoric acid traces.
-------
100·00

Green ultramarine is transformed into blue by heating with about 4
per cent. of sulphur at a low temperature, with free access of air.
Sulphur is afterwards added, if necessary, in small quantities at a
time, and the heating is continued until the desired shade of blue is
obtained. The mass is then powdered, the soluble matter (sulphide of
soda, &c.) is removed by washing with water, and the blue is dried and
assorted according to quality.

(_b_) “_Soda_” _Ultramarine_ is sometimes made with soda alone (either
carbonate or caustic), and at others with a mixture of soda and
sulphate of soda. Rowland Williams found the following proportions of
the respective ingredients to answer satisfactorily:--

Per cent.

China clay 36·8
Carbonate of soda 36·8
Sulphur 22·0
Coal 4·4
-----
100·0

The proportions for soda and sulphate of soda ultramarine have been
previously given under “sulphate ultramarine.” The ignition is carried
on in a manner similar to that already described. The resultant
green product, owing to its avidity for oxygen, is partially changed
into ultramarine blue by simple contact with the air. It is entirely
converted into the blue variety by roasting with an additional quantity
of sulphur. With care, ultramarine blue may be manufactured in one
operation, by increasing the proportions of soda and sulphur.

(_c_) “_Silica_” _Ultramarine_ is manufactured in the same way as soda
ultramarine, except that, in addition to the other materials, silica to
the extent of 5 or 10 per cent. of the weight of clay is employed. By
this process, ultramarine blue of a slightly reddish tint is obtained
in one operation. The method has, however, one decided drawback, viz.
that the materials employed are rather liable to fuse during ignition.
The faintly reddish hue of “silica” ultramarine becomes more intense
according to the proportion of silica present. “Silica” ultramarine
is said by some to be less readily attacked by acids and by strong
alum solutions than ultramarine prepared by the “sulphate” and “soda”
processes; but Rowland Williams’ experience does not confirm this
statement. He mentions that good artificial ultramarine withstands
the action of weak acids much better than is generally imagined. He
had occasion to test many samples which resisted the action of dilute
acids to a remarkable degree. Most strong acids, of course, decompose
both artificial and native ultramarine, with evolution of sulphuretted
hydrogen. Native ultramarine is, however, less susceptible to the
influence of acids (both strong and dilute) than the artificial
compound. This difference of behaviour is probably due to the fact that
the former contains considerably less sulphur than the latter, and it
is also possible that the constituents of natural ultramarine may be
combined in a somewhat different manner from those of the artificial
product.

Notwithstanding the large amount of research with reference to the
chemical composition of ultramarine, the origin of its blue colour
still remains in doubt. According to Wilkens (_Ann. Ch. Pharm._, xcix.
21), ultramarine consists of two portions, one of which is easily
attacked by hydrochloric acid, and is regarded by him as the essential
constituent, whilst the other portion is insoluble in hydrochloric
acid, and contains variable proportions of clay, sand, oxide of iron,
and sulphuric acid. From his analyses of the pure blue, Wilkens
deduces the formula (2Al_{2}O_{3} 3SiO_{2}) (Al_{2}O_{3} 4SiO_{2})
Na_{2}S_{2}O_{3} 3Na_{2}S:--

Per cent.

Silica 37·6
Alumina 27·4
Sulphur 14·2
Soda (Na_{2}O) 20·0
----
99·2

Wilkens regards the blue colouring principle of ultramarine as a
compound of hyposulphite and sulphide of sodium. He considers the
presence of iron is not necessary for the production of the blue;
whilst Dr. Elsner, in a paper published in 1841, states that about 1
per cent. of iron (which he presumes to be in the state of sulphide)
is essential. Rowland Williams asks whether it is not conceivable
that the blue colour of ultramarine may be due to the presence of a
small quantity of black sulphide of iron, most intimately combined
with a colourless or comparatively colourless compound (such as white
ultramarine), the whole mass (owing to the dilution of the black
sulphide) showing a blue reflection.

Ultramarine is insoluble without decomposition in any known menstruum.
According to P. Ebell (Ber. 16), ultramarine, when in the most finely
divided state, will remain suspended in pure water for months. The
liquid may be filtered unchanged through several layers of Swedish
filter paper, and appears perfectly clear when examined in a ¾ in.
layer, and on evaporation deposits the ultramarine as a lustrous
coating on the sides of the vessel. Rowland Williams repeated the above
experiment, and can confirm Ebell’s statement. This result shows the
necessity of due precautions being taken during the washing of the
ultramarine in the process of manufacture, otherwise a considerable
amount of the finely divided blue may be lost. Ultramarine is largely
used in calico printing for pigment styles, being fixed on the fibre
by means of albumen. It is also employed for blueing linen and cotton,
wax candles, lump sugar, &c. Ultramarine is not adulterated to a large
extent, the chief sophistication being barium sulphate (barytes), and
occasionally chalk and china clay.--(Rowland Williams, in _Industries_.)

Another writer in _Industries_ says that the manufacture of ultramarine
has perhaps hardly received the attention it deserves in England. The
importance of the industry has been recognised in Germany, however,
and though the palmy days of the trade, when the whole production was
in the hands of a few firms, and the price was a matter of private
friendly arrangement, are gone for ever, yet the business is in a
flourishing state, and should prove lucrative if properly managed.
It is a characteristically English failing to overlook branches of
business not dealing with large quantities of staple commodities, and
thus many of the smaller but remunerative industries have passed out of
our hands. When one observes that almost every sheet of ordinary blue
official paper is decolorised when accidentally brought into contact
with an acid, betraying the fact at once that its colouring matter is
ultramarine, one realises that a very considerable consumption for
this and similar purposes must take place. Like most trades based upon
chemical principles, the manufacture of ultramarine has recently made
rapid strides, and some of the latest developments are recorded in
a paper by J. Wunder, appearing in a recent number of the _Chemiker
Zeitung_, which is worthy of some attention.

With most people not directly interested in it, the term ultramarine
is taken to mean the _blue_ pigment known under that name, the words
being reckoned almost synonymous. Others, more erudite, recognise the
existence of a green variety, but that the production of such colours
as red and violet is possible is scarcely suspected. Of course the
blue is the most important, but even that does not correspond to one
specific substance, products of different shade being prepared by
modifying the process of manufacture. As usually made, ultramarine is
formed by heating together carbonate of soda, kaolin, sulphur, and
charcoal, with limited access of air, the resulting pigment being
green; this, on roasting with sulphur, becomes blue. If the operation
be conducted with complete exclusion of air, so-called ultramarine
white (in reality _grey_) is produced, which becomes green on further
heating. Ultramarine blue capable of resisting the action of alum
is sometimes required, and may be obtained by the use of a highly
silicious charge and much sulphur, the burning being conducted in
crucibles or in mass according to the purpose for which the pigment
is required. The former process is costly, while the latter gives a
product containing a good deal of free sulphur, which is objectionable
for such purposes as calico printing. Removal of the excess of sulphur
by heat or caustic soda is not feasible, as the colour suffers in
either case, but a certain amount of success has attended experiments
with sodium sulphide, the colour often brightening noticeably.

It is curious that chemically pure sodium carbonate, or such as is made
by the ammonia-soda process, is not well fitted for the manufacture of
ultramarine; Leblanc soda, containing a little caustic, is distinctly
preferable. Sprinkling the soda with a strong solution of sodium
sulphide before use is a good plan, and one easy to adopt. The more
silicious the mixture the more difficulties are encountered, but the
product is a deeper, richer colour, and withstands the action of alum
and weak acids better. Excess of oxygen must be guarded against; many
a manufacturer has had a batch turn out a hard cold blue, instead of
a soft rich colour, solely on account of a too-excellent draught,
an accident especially liable to happen in winter time. So much
dreaded is this catastrophe that some makers habitually limit the air
supply--smothering the neighbourhood with smoke, and wasting coal. The
need for exact control here indicated points to a probable advantage
from the use of gaseous fuel. Considerable economy has resulted from
the use of the waste gases from one furnace serving for the preliminary
heating of another; a better plan would probably be the introduction of
regenerative heating.

The crude ultramarine as it comes from the furnace contains a large
proportion of soluble salts, notably 20 to 24 per cent. of sodium
sulphate, which have to be removed before it is merchantable. Usually,
after grinding, it is simply stirred up repeatedly with hot water and
the aqueous extract is siphoned off. That such a crude method should be
in vogue at the present time is very significant of the ample margin
of profit that must exist. By systematic extraction and filtration
under pressure the washing may be effected with so little water that
the solution is sufficiently concentrated to pay for evaporation by the
heat of waste furnace gases, the recovered sodium sulphate serving to
replace part of the raw material.

The quality of ultramarine largely depending upon its fineness, it
is graded by levigation, the coarser portions being filter pressed,
and the finest “floating” quality, which remains in suspension for an
inconveniently long time, precipitated by the addition of a trace of an
ammonium salt, gypsum, or even hard water, and filtered by the aid of a
suction tube on the principle of an ordinary Bunsen pump.

The first successful attempt to produce ultramarine _violet_ was made
by Professor Leykauf in 1859. By heating ordinary ultramarine with
calcium chloride in the presence of air and moisture, he obtained
a violet-toned pigment, but it was not a full colour. The active
substance in this change was probably hydrochloric acid, produced by
the decomposition of the calcium chloride. Later experiments with
other reagents, such as chlorine and gaseous hydrochloric acid, led to
the following methods being devised. In the first, ultramarine blue
is spread out on stoneware shelves in iron chambers and treated with
a mixture of chlorine and steam at a temperature of 300° F. to 480°
F. for about three hours. In the second, the plant is very similar,
but at the bottom of the chambers are stoneware dishes, into which
hydrochloric acid is poured from time to time. As the temperature is
raised, copious vapours arise from these, evaporation being aided
by a strong draught, and the ultramarine blue, after being kept at
428°-446° F. for some seven hours, becomes converted into a dull
violet, which brightens on continuing the process with a temperature
gradually falling to 320° F. The ultramarine violet produced by either
of the above methods resists the action of lime, and is of general
applicability.

The pigment produced by a third and simpler process, consisting merely
in heating ultramarine blue mixed with salammoniac and a little
sodium nitrate, is unfortunately not so stable. Another shade of
considerable interest is a pure bright light blue, formed by heating
the violet variety in hydrogen to about 536°-554° F. It has not yet
been prepared on a commercial scale, but certainly merits the attention
of manufacturers. An ultramarine red has been made by acting on the
violet produced by either of the first two methods with the vapour of
either nitric or hydrochloric acid at 275°-293° F., the sole essential
determining condition being the temperature. Iron vessels could be used
in the case of nitric acid at this temperature, but if hydrochloric
acid were employed stoneware would have to be substituted. In the
manufacture of the violet the temperature is above the limit at which
hydrochloric acid acts on iron.

It is now only necessary for some successful experimenter to put on the
market yellow and orange shades of ultramarine for almost the whole
of the spectrum to be represented. The problem of the cause of the
colour of ultramarine, attempts to solve which have been repeatedly
made, seems increasingly difficult when its protean character is
considered; but this from the industrial point of view is of secondary
importance, provided all required shades can be produced with ease and
economy. Nevertheless, it is certain that here, as in other cases,
substantial technical progress would follow from adequate scientific
investigation.--(_Industries._)

Ultramarine was also made the subject of a very interesting paper, by
Herbert J. L. Rawlins, read before the Society of Chemical Industry, in
December 1887.

After referring to the native form, lapis lazuli, Rawlins goes on
to observe that “analysis could give no clue as to the cause of
the blue colour. To prepare it artificially became a great object,
and the efforts in this direction were stimulated by the offer of
prizes, amongst which was one of 6000 francs, offered by the ‘Société
d’Encouragement’ of France, to be awarded to the discoverer of a method
of making ultramarine, provided it did not cost more than 90_s._ per
lb. How strange it seems to think of this in these days when the value
has fallen to less than half that price per cwt.!

“As early as 1814, two German chemists, Tessärt and Kuhlmann, had
observed the formation of a blue product in soda kilns and calcination
kilns, but Guimet, in 1828, first discovered how it was produced, and
gained the 6000 francs prize. He did not, however, publish his method,
and grew immensely rich, although the price sank to about 16_s._ per
lb. In 1828 he was producing at the rate of 120,000 lb. annually.

“About the same time, or, as is positively asserted by some, even prior
to Guimet, Gmelin made the same discovery and published his researches
in full, thus perhaps laying the foundation stone of the present
supremacy of Germany in this manufacture.

“In spite of the valuable discoveries of Hoffmann, Unger, and others,
our knowledge of the chemical constitution of ultramarine is very
limited and uncertain, many different theories having been advanced
regarding the cause of the blue colour.

“According to Wilkins, ultramarine is composed of two portions, one
of which consists of two silicates of alumina with sulphite and
sulphide of sodium, and is constant in its composition; the other
being a mixture of variable quantities of sand, clay and oxide of
iron, with sulphuric acid. The blue colouring principle he considers
to be a compound of sodium sulphite and sulphide. Another ingenious
theorist, Stein, in two papers published in the _Jahresberichte_ in
1871 and 1872, concludes that blue ultramarine contains sulphurous,
and not thiosulphuric acid, that neither sulphites nor thiosulphates
are necessary to its composition, and that it owes its colour to
the presence of black sulphide of sodium, which is formed at high
temperatures by the action of sulphide of sodium on alumina--admitting,
therefore, that it is not a chemical compound, but merely a mechanical
mixture, the blue colour of which is due to the bodies composing it.

“Brunner considers ultramarine to be a compound of aluminium silicate,
with sodium sulphate and sulphide; while Brünlin regards it as a double
silicate of aluminium and sodium, in combination with pentasulphide of
sodium. Green ultramarine he considers to be the same double silicate
in combination with bisulphide of sodium.

“Again, according to Ritter, ultramarine contains a double silicate,
not only associated with polysulphide, but also with thiosulphate of
soda; and Schülzenberger, on the other hand, considers that it is a
mixture of a double silicate with sulphite and monosulphide of sodium.

“Endemann considers that the blue colour is due to a ‘colour nucleus,’
consisting of unchanging proportions of aluminium, sodium, oxygen and
sulphur, in each variety of ultramarine the proportion being different,
while the rest of the sodium and aluminium and the whole of the silica
merely act as a vehicle necessary to the preparation and existence
of the colour. He considers that this ‘colour nucleus,’ in the case
of white ultramarine, which he calls the ‘mother-substance in the
manufacture of blue ultramarine,’ has the formula AlNa_{4}O_{2}S_{2}.
By the action on two molecules of this of sulphurous acid gas,
Na_{2}O is removed, and green ultramarine Al_{2}Na_{6}O_{3}S_{4}
is formed, which then, by the action of oxygen, which forms sodium
sulphate, passes into the pure green compound, having the formula
Al_{2}Na_{4}O_{3}S_{3}. In the ‘indirect process’ of manufacture, green
ultramarine is converted into blue by being burned with sulphur. By
this means Endemann considers that more sodium and sulphur are removed,
and blue ultramarine Al_{2}Na_{2}O_{3}S_{3} is formed. He considers
that the other portion, not included in the ‘colour nucleus,’ differs
in different samples. In one which he mentions it has about the
composition 3Al_{2}O_{3}.5Na_{2}O.16SiO_{2}.

“But of all chemists who have worked on this subject, none has done
more to increase our knowledge of ‘the blue marvel of inorganic
chemistry,’ as he himself has called it, than Reinhold Hoffmann.
His position of manager of the Marienberg Ultramarine Works, near
Benscheim, in the Grand Duchy of Hesse, renders his acquaintance with
the manufacture perfect, and his untiring researches on the subject
have been well rewarded by results both interesting and valuable.
He considers ultramarine to be a double silicate of sodium and
aluminium, together with bisulphide of sodium, the variety poor in
silica, characterised by its paleness and purity of tint, and easy
decomposition by acids, having the formula 4(Al_{2}Na_{2}Si_{2}O_{8})
+ Na_{2}S_{4}; while that rich in silica, characterised by its dark
and somewhat reddish tint, and more difficult decomposition by acids,
has the formula 2(Al_{2}Na_{2}Si_{3}O_{10}) + Na_{2}S_{4}. He also
considers it very doubtful whether green ultramarine is really a
chemical compound, and indeed it is now generally considered that the
colour is only due to small traces of sodium salts in very intimate
mechanical mixture with the blue variety, for by heating the green
body for some time at 160° with water in closed tubes, it is converted
into the blue product, and small traces of sodium compounds are found
in solution in the water; and further, on heating blue ultramarine
strongly with sodium sulphate and charcoal--that is, acting upon it
with sodium sulphide--the green variety is formed.

“In a paper by Knapp, an abstract of which appeared in the _Journal
of the Chemical Society_ for March 1880, there are some curious facts
recorded with regard to the colouring agent. It was noticed that when
silicic acid was replaced by boracic acid, a blue, nearly as stable in
its properties as that of ordinary ultramarine, was produced. It was
found that a blue could be obtained without alumina being introduced.
Hence silica without alumina, and alumina without silica, can be
employed with a certain amount of success. The blue, however, formed
without silica, is not so strong or stable as that formed with it.

“One very curious property which ultramarine possesses is its power of
giving up its sodium in exchange for other metals. Thus, by heating
blue ultramarine with a concentrated solution of silver nitrate
in sealed tubes to 120° for fifteen hours, a dark yellow _silver_
ultramarine is produced, containing about 46·5 per cent. of silver.
This corresponds to about 15·5 per cent. of sodium, which is just about
the amount that the original body contained.

“When this body is heated with an aqueous solution of sodium chloride
to 120° in sealed tubes, about three-quarters of the silver is replaced
by sodium, but the other quarter cannot be so replaced; in fact, blue
ultramarine, when heated with silver chloride, takes up silver, and
becomes green. But by heating silver ultramarine with sodium chloride
in the dry way, at rather a higher temperature, the whole of the silver
is replaced by sodium, but the ultramarine thus regenerated does not
equal the original body in colour. The change is probably due to the
loss of sulphur in the formation of the silver ultramarine.

“If in the above experiment potassium chloride be substituted for
the sodium salt, and the temperature not allowed to exceed 400°, a
bluish-green _potassium_ ultramarine is formed. _Barium_ ultramarine
is a yellowish-brown product, _zinc_ ultramarine is violet, and
_magnesium_ ultramarine is grey. These may all be obtained by acting on
the yellow silver ultramarine with the corresponding metallic chloride.

“From the experiments of Dollfus and Goppelsröder some very striking
differences have been brought to light between the three types of
colour which they examined--namely, the blue, green and violet--in
their behaviour with various reagents. Thus, an aqueous solution of
caustic soda or potash does not act on the blue or green, but turns
the violet to blue, and when heated with carbonic oxide the same result
ensues. Many other reagents have the same effect on the violet variety,
but when acted upon with sodium sulphide, the green turns grey, and
when heated with potassium chlorate becomes darker and loses its
brightness of colour. Dollfus and Goppelsröder attempt no explanation
of these facts, but simply state them as results of their observations,
and profess their inability to give any chemical formulæ for the three
ultramarines, though they consider that there is sufficient proof
that each has its distinct constitution. They give as their opinion,
however, that they are double silicates of aluminium and sodium, in
which a part of the oxygen is replaced by sulphur.

“Violet and red ultramarines are more bodies of scientific interest
than of any practical use, as their colouring power is not sufficiently
great. The violet variety may be prepared by exposing the underground
blue product to chlorine gas under a high temperature, while the
red may be obtained from the violet by acting on it, under a low
temperature, by dilute nitric acid fumes.

“The first artificial method of producing ultramarine was that known
as the ‘indirect process’--that is, first the manufacture of green
ultramarine; and secondly, its conversion into blue. It was carried out
as follows:--

“An intimate mixture of Glauber’s salts, china clay, and coal or rosin,
finely ground together, was placed in crucibles and baked or burned in
an oven for about six hours. It was then transferred to iron trays,
and heated with flowers of sulphur to the point where the sulphur took
fire, when it was allowed to burn itself out. By this second process
the green was converted into blue. It was then washed, ground with
water, and settled out, the first deposit being of a darker shade than
the second, and the colour becoming lighter as the powder settled was
finer in grind. This is essentially the method employed now at many
German works--those at Marienberg, for instance--and produces what is
known as “sulphate ultramarine,” distinguished by its pale shade and
almost _greenish_ blue tint.

“There are, however, some objections to the indirect process, and it
was considered advisable to find a plan by which ultramarine could be
made in bulk in a muffle furnace. The following is a method which is
employed at the present time in some of the German works:--

“A mixture of china clay, carbonate of soda, sulphate of soda, sulphur,
sand and charcoal or rosin, finely ground together, are placed upon
the floor of a muffle furnace, being pressed down so as to present an
even surface. The mixture is then entirely enclosed with fire-clay
tiles, the spaces between which are filled in with thin mortar. When
the oven is so charged, the front is built up, a small hole being left
for watching the temperature of the flue between the tiles and the top
of the furnace, and for drawing samples during the process, which is
done through a corresponding hole in the front of the fire-clay tiles,
temporarily closed with a fire-clay stopper. The oven is now heated,
slowly at first, and afterwards more strongly, so that at the end
of eight or nine hours it is at a dull red heat. It is kept at this
temperature for about 24 hours, when the heat is raised so that a clear
red glow is obtained, which is kept up to the end of the operation.

“For the purpose of taking a sample, an iron spoon borer is introduced
through the hole left in the enclosing tiles, turned round, and pulled
out. The contents are laid on a clean tile, and quickly covered with
another tile, on which a second quantity is placed, and allowed to
remain exposed to the air. If the oven has been sufficiently heated the
covered sample should appear of a bluish green, and no longer brown
or yellow, while the second sample should be rather bluer. If this be
the case, the oven is heated slowly for another hour, and then all
communication with the outer air is cut off. It is allowed to cool and
then opened, when the contents should appear as a beautiful blue mass,
the lower portion of which, however, is of a greenish tinge. Both parts
are now treated alike, but worked up separately, the greenish-blue
portion making an inferior article. The finishing process is as
follows:--

“The raw ultramarine is ground in upright mills, and then repeatedly
boiled for about ten or fifteen minutes at a time in cast-iron boilers,
being all the time agitated by a mechanical stirring arrangement. It
is then allowed to settle, and the water is drawn off with a siphon.
As soon as the powder settles into a hard compact mass, it has been
sufficiently washed, and it is then dug out. The part next to the
bottom of the boiler is generally coarse and of poor quality. It is
carefully separated from the upper portion, which is transferred to wet
mills of the ordinary description, and there ground for six to twelve
hours, during which time about 150 lb. can be treated in each mill.
The ground colour from these mills is then collected in a large tub,
and allowed to settle for four hours, during which time the coarsest
particles fall to the bottom. The liquid is then passed through a
series of tubs, in each of which it is allowed to stand for a period of
time, lengthening as the quality settled out becomes finer, the last
settling requiring about three weeks. The various qualities are then
dried and sifted, when they are ready for the market.

“The blue produced by this operation is of a good quality, but there
are some objections to the process, which have given rise to another,
in which the ultramarine is produced direct in crucibles similar to
those used in the indirect process.

“This is conducted as follows:--The mixture of raw materials consists
of about 100 parts of china clay, 90 of carbonate of soda, 110 of
sulphur, 20 of charcoal, and a quantity of infusorial earth, varying
according as the ultramarine produced is desired to be rich or poor in
silica. These are finely ground together, in which process great care
must be observed, as much depends upon its being properly carried out.
The mixture is then filled loosely into crucibles provided with flat
circular lids, which are fixed on with mortar containing clay. This
is allowed to dry, and the crucibles are then ready for firing, which
process is conducted in ovens, generally constructed so as to contain
several hundred crucibles, which are arranged in rows one above another.

“The mixture undergoes a very curious change of colour while in the
ovens. When put in it is greyish white, and during the process of
burning it becomes successively brown, green, blue, violet, red and
white, in the order named. These changes are, according to Guimet,
due to oxidation. The brown appears with the blue flames due to the
combustion of the sulphur, the green just after the sulphur flames have
ceased, and the blue is first formed at a temperature of about 700°--i.
e. a bright red heat. If, after this, heat be still applied and air
freely admitted, the mixture becomes first violet, then red or rose
coloured, and finally white. When this white body is heated to redness
with carbon or other reducing agents, the red, violet, blue, green and
brown colours (according to the amount of reducing agent employed) may
sometimes be reproduced, though the reaction is by no means a certain
one.

“If brown ultramarine be removed from the oven, and allowed to remain
exposed to the air, it immediately takes fire and burns to an inferior
blue colour. The same thing occurs with the green body. Even if the
brown product be completely cooled before being exposed to the air,
it will, as soon as the air is allowed to reach it, get hotter and
hotter, until it is glowing, when it will burst into flame and become
blue. Attempts have been made to preserve the brown colour, which is of
a beautiful chocolate tint, but have always failed. In one instance,
when this was tried, the colour was put immediately into water, and
treated like the ordinary blue variety, and as long as it was kept
moist no change was apparent. After being washed and wet ground the
moist powder was put into a cask, where for some time it was allowed to
remain undisturbed. At the end of about three weeks it was noticed that
the mass was hot, and on being turned out of the cask and broken up it
was found to be at a glowing heat in the interior.

“After the oven has been fired for several hours, it is carefully
closed at every point where air might enter, and allowed to cool
for four or five days. The exact length of time during which the
ovens are fired, and the amount of air admitted, depend upon various
circumstances, one important one being the state of the weather. Thus,
on a dull, foggy day, when the draught in the chimney is not good, a
longer time is required. Of course, no rule can be given for this,
and it is the experience required in the management of the oven that
makes the manufacture so difficult to carry out successfully, the early
efforts of a manufacturer not unfrequently resulting in the loss of
a whole ovenful of raw material. As soon as the oven has cooled, the
crucibles are taken out, and the contents of each are turned out in a
solid mass, which must be carefully cleaned with a knife of any badly
burned portions, and afterwards broken up and thrown into a cask along
with the contents of other crucibles.

“This forms what is known as crude raw ultramarine. It contains about
15 per cent. of sulphate of soda, which must be removed before the
colour is fit for sale.

“For this purpose it is washed with hot water in large tubs, after
which it is ground in wet mills to an impalpable powder, and allowed
to stand for about an hour in a large tub, in order to remove the
coarsest particles and dirt which are sure to be present. It is then
removed to another tub, where it settles for four or five hours, and
from this it passes to others, where it stands for various lengths of
time, increasing, of course, as the powder to be settled becomes finer,
the last settling occupying three or four weeks, and producing the
strongest quality that can be obtained--that is to say, it will bear
mixing with more of a reducing medium, such as mineral white, than
would a former settling for the mixture in each case to be of the same
depth of colour.

“The water, after the final settling, still contains about 5 per cent.
of ultramarine. This would take five or six months to settle, and
as this time could not generally be given to it, it is precipitated
with lime water, which has a sort of coagulating influence upon the
particles, which can then be removed by filtration. It is a curious
thing that this last quality is quite different from the one preceding
it, being very inferior in both colour and strength.

“After settling, all the various qualities are dried in kilns, and
sifted through fine brass wire sieves by means of a fan, which breaks
up the lumps and forces the particles through the meshes of the sieve,
which must be very close--about 100 to the inch--in order that the
ultramarine may be perfectly smooth and free from lumps or grit of
any sort. When finished, it should be in the form of an impalpable
powder--the finer qualities so fine, indeed, as to feel almost
_buttery_ when rubbed between the fingers. After this process the
different qualities and shades are mixed to certain standards, and are
then ready for sale.

“The uses of ultramarine in the arts and manufactures are very numerous
and important. The most important, from the point of view of quantity,
is the manufacture of ‘square blue’ for washing purposes. In the
preparation of this article the ultramarine is generally mixed with
bicarbonate of soda and some glutinous material, to help it to retain
its shape, and is then pressed into the well-known form of small square
or oblong blocks.

“It is also used largely in the manufacture of blue paint and printing
ink, and in the preparation of blue mottled soap. The way in which it
is employed in the last-named manufacture is worthy of remark. It is
added to the soap while it is in a molten state and just before it
is allowed to cool, and thoroughly mixed with it, so that the whole
mass is of a pale blue tint. If a small quantity of this be removed
from the boiler and cooled quickly, it remains of a uniform tint, but
in the case of the whole boilerful, where the cooling is very slow,
the action is entirely different. Just at the point of cooling, when
the soap is going to set hard, the ultramarine--to use a technical
expression--“strikes,” and goes into the form which gives to blue
mottled soap its well-known appearance.

“In the manufacture of paper, ultramarine also plays an important part.
It is here used not only for producing blue shades, but also as a
bleaching agent, to counteract the yellow when white paper is made.

“Another important use is in the calico manufacture, where it is used
both in the printing of blue patterns and in the finishing of goods. In
the case of calico printing, it is mixed with albumen and printed on to
the calico, which is then subjected to the action of steam, the albumen
being by this means coagulated and each grain of ultramarine surrounded
by an insoluble envelope, so that it cannot be washed out of the calico.

“The growth in the manufacture of ultramarine has been very remarkable,
especially when it is considered how little the process is understood
chemically, and what care and patience--to say nothing of the
equally important item of capital--are required in the starting of
a manufactory. Commencing less than 50 years ago in the works of
Guimet, at Lyons, who produced 120,000 lb. annually, there are at the
present day nearly 40 manufactories at work in various parts of the
world--chiefly in Germany--producing about 20 million lb. per year.
The following figures will give some idea of ten years’ growth of this
industry--from 1862 to 1872:--

1862. 1872.

Number of manufactories 24 32
Men employed 964 1929
Tons manufactured 3556 8585

“From the above numbers it will be seen that in these ten years the
manufacture more than doubled itself, the fact being due, however,
not so much to the increase in the number of works, which was only
one-third, as to the enlarged capabilities of those existing in 1862.
Thus, in the works of Dr. Leverkus, near Cologne--the first works ever
started in Germany--the number of men employed had, during these ten
years, more than doubled, while the output had trebled; and in the case
of the Marienberg Works the difference was even more striking, the
number of hands employed and the quantity turned out per annum having
nearly quadrupled.”

In reply to various questions which were asked in the discussion which
ensued, Mr. Rawlins said that, with regard to the use of ammonia
soda, it had frequently been used in the manufacture of ultramarine,
and was constantly used he understood, but he himself had not much
experience of it. As far as he could make out, it certainly produced
ultramarine, but of a darker shade than that made with Leblanc soda.
It could not be supposed, in works where the Leblanc soda was used,
that ammonia soda could conveniently be substituted, for of course
a works when established had to adhere to its known standards and
shades, and it would not do to change the raw materials, though the
ammonia soda produced a very good ultramarine. As regards the discovery
of ultramarine, the first works started anywhere were Guimet’s. He
had with him a little historical list containing the dates at which
the various works established before 1866 or a little later had been
started. It was drawn out by Hoffmann, who, as he stated before, was
the manager of large ultramarine works, and he put down Guimet’s,
which were started in 1829, first on the list. Dr. Leverkus started in
1834. He knew that the discovery of ultramarine had been attributed
to different people. He had mentioned Guimet because it had generally
been considered, as far as he had heard, that Guimet and Gmelin were
the two who discovered it from a manufacturing point of view. He had
heard of crystals of ultramarine, but had never seen any, and he knew
they were very difficult to prepare, and very rare. He had mentioned
that the grinding had to be done very thoroughly, because the better it
was mixed and the finer it was ground, the better was the ultramarine
produced. If it was badly mixed it was quite fatal to getting a good
result. Grinding lightens the colour. Raw ultramarine must be ground
before it was practicable to use it at all. For instance, a coarse
ultramarine could not be used for printing calico. Therefore it was
necessary to grind it both for the sake of the colour and for the
sake of the way in which it was applied. It was increased in value by
grinding because it made it stronger and finer. Before grinding it was
of a dark colour, but after grinding it became lighter and brighter.

The materials employed in McIvor’s process for making ultramarine
are kaolin or other suitable clay, a solution of sulphide of sodium,
in which sulphur in the form of flowers of sulphur is dissolved to
saturation, and caustic or carbonate of soda.

The preparation of the solution is effected by adding the sulphur to
boiling sulphide of sodium liquor of maximum strength until it ceases
to be taken up. The clay and soda are first roasted together at a red
heat, so as to effect a partial double decomposition, and the product,
after grinding, is made into a thick paste with “sulphur liquor,” i. e.
the sulphide of sodium solution of sulphur. This latter operation may
be carried out in an ordinary pug-mill. The paste so formed is dried in
an oven or other convenient way, and the dried mass (being broken into
small pieces) is roasted without access of air in a closed earthenware
retort, first at about 480°-570° F. for an hour, then at a red heat for
eight hours, and finally at a moderate heat just below dull redness,
in presence of a slow current of air, which enters through a series of
holes or small openings in the front of the retort, the current being
regulated by means of a damper or an adjustable slide. The retort
should be allowed to become quite cold before being opened, otherwise
the tint of the product will be injured.

McIvor has found the following proportions of the raw materials used in
the process to yield excellent results, viz:--

Sulphide of sodium 42 lb.
Sulphur 20 “
Kaolin (china clay) 110 “
Soda (as carbonate) 106 “
or
Caustic soda 40 “

These quantities yield about 2 cwt. of ultramarine blue.

The following communication from the pen of J. B. Nejedly, of Vienna,
appeared in the _Chemiker Zeitung_, during 1888:--

“Animated by various articles and notes in your journal under the
heading of ‘The Present Position of the Manufacture of Ultramarine,’
I would like to draw out of obscurity a little work on this industry
which contains much that is true, and furnishes at the same time many
comparisons with regard to the present position of the ultramarine
industry in Germany.

“The work above referred to was printed in the year 1840 and bears the
title:--

“‘Treatise on the chemico-technical preparation of Ultramarine
colours, according to the discoveries of Leykauf and Heyne, or on
the importance of the manufacture of blue and green Ultramarine for
purposes of science, art, and industry. By Friedr. Wilh. Heyne,
president of the Nürnberg Ultramarine Manufactory. Nürnberg: 1840.
Printed at the Campe Press.’

“The preface, which I consider to be well suited to present
circumstances, I reproduce verbatim, while from the little work itself
I will only quote such sentences as would seem to be suited to the
present time, and which are the most important as bearing on the
subject.

“‘_Preface._--The incitement to this treatise was furnished by the
utility of the discovery of Leykauf, instructor of chemistry at the
technical schools in Nürnberg, of artificially preparing the well-known
blue mineral colour styled ultramarine, according to simple principles,
which discovery was supplemented by the production of the green
ultramarine, an equally genuine and beautiful green mineral colour,
by the technist Heyne in Nürnberg. A short review of the importance
of these two discoveries for mankind in general and for science,
art, and industry in particular, will form the main subject of this
treatise, which has no other object but that of arousing the attention
of all high protectors and stimulators, as well as friends of industry
and art, to a newly-born industrial branch. At this moment we are
living in a period when many industries have got into the stocks,
in consequence of far too severe competition, combined with other
influences; indeed they are barely able to support those engaged in
them. If in consequence of this state of things it already becomes of
the most vital importance that fresh sources of acquisition should be
obtained, it becomes all the more so when by their means at the same
time materials come into requisition which the Fatherland possesses
in great superfluity, and which otherwise possess no intrinsic
value beyond just the expense of extracting them from their natural
localities or deposits, and the worth that attaches to their working up
for industrial purpose. A source of acquisition in this sense is met
with in the manufacture of blue and green ultramarine colours, which in
course of time can be raised to an extremely valuable acquisition. May
the communications here made result in their being considered worthy of
a thorough many-sided investigation and consideration.’

“REGARDING THE WORK ITSELF.

“Page 21.--‘Not long since a prize of 6000 francs was offered by the
“Société d’Encouragement.” This prize was gained by Guimet, who has not
published his process, and who now furnishes ultramarine at the price
of 25 francs per oz., whereas it otherwise cost 200 francs per oz.
Latterly, in 1839, Guimet reduced his price for ultramarine, viz. No.
1, for painting, to 10 francs, a lighter shade being 6 francs per oz.
In addition, this manufacturer furnishes lower qualities for carpet and
paper manufacturers at 20 francs and 12 francs per lb.’

“Page 23.--‘Indeed, if we are able to produce ultramarine by means of
a polysulphide of sodium and common clay, then the most beautiful and
most lasting of all known blue colours would at the same time become
the cheapest of them all.’

“Page 27.--‘All faults which are known to exist in the old methods are
obviated in the new invention of Leykauf and Heyne, while the same
offers the following advantages:--

“‘(1) The materials which are treated with it can be brought into use
without any special previous chemical preparations, indeed as supplied
by Nature, while chemical treatment is entirely unnecessary. In view of
the unimportant cost of derivation of the raw material, there cannot
consequently be any questions raised with regard to waste.

“‘(2) This method is so simple that any man of sound intellect can
easily work it, without possessing any special chemical knowledge
beforehand. As the labour can be easily grappled with, errors can only
occur when the grossest carelessness is shown in conforming to the
instructions prescribed.

“‘(3) According to the said method one can work according to any
desired scale, and, what is best of all, the larger this scale the more
favourable are the results obtained, lighter work and excellence of
quality.

“‘(4) If the process is carefully conducted, everything is in your own
power, nothing depending on chance.

“‘(5) Consequently an equal product can invariably be obtained, while
this can at will be brought to the most complete stage of perfection
at but little greater cost than lower qualities entail.

“‘(6) According to this method you are master of the fire, enabling a
retention of colours in any desired shade, of the deepest tone, of the
greatest permanency.

“‘From this it appears: That this process is the easiest, the cheapest,
and the most complete. Worked according to this method the hope is
likely soon to become a reality that ultramarine may yet become the
cheapest of all mineral colours, and as in the same everything rests
upon simplicity, the preparation of the article in future will be
carried on somewhat after the fashion of baking, brewing, &c.’

“Page 32.--‘Moreover, there is not only blue ultramarine, but also a
pure green, and we may venture the hope that similar combinations in
white, black, red, and yellow will soon follow in equal perfection.
In consequence of these discoveries, Leykauf and Heyne have erected a
factory in Nürnberg, which, according to a circular dated 15th July,
1840, is in operation under the style of “Leykauf, Heyne and Co.,” and
are producing the two ultramarine colours referred to at the present
time at the rate of 50 lb. per day.’

“Page 33.--‘All the mechanical appliances of the factory are at the
present time exclusively worked by hand, the number of persons employed
being sixteen; while the establishment upon completion of the buildings
that are wanting is calculated to employ twenty operatives and two
horses. With this extension the factory will be able to turn out 5
cwt. blue and 5 cwt. green weekly, consequently annually 500 cwt. of
finished merchantable ultramarine will be brought on the market.’

“Page 35.--‘Now, as regards the prices ruling at present for Nürnberg
ultramarine, these are, as compared with those of the French, more than
500 per cent. cheaper. Blue ultramarine costs, namely, in Nürnberg,
quality No. 0, 10 florins per lb.; a lighter quality, which is
nevertheless darker than the darkest French at 100 francs, 5 fl. per
lb.; a third quality likewise darker than the seconds French at 60
francs, 3 fl. per lb. Green ultramarine, 3 fl. 10 kr. per lb.

“‘How much further, however, these low prices will be yet reduced
after the completion of the factory, may be gathered from a detailed
calculation of cost which the chief of this factory has made himself
responsible for as being the highest estimate. This calculation of
cost is based upon the weekly production of 10 cwt., which the factory
will soon be able to turn out, and upon a necessary cost of plant and
working capital of 90,000 Rhenish florins, as follows:--

“Page 36.--‘Calculation of cost of 500 cwt. blue and green
ultramarine:--

Fl.

(1) Raw material and cost of transport 10,000
(2) Fuel, including cost of transport of 7200 cwt. of
coal at fl. 1.30…

source: Project Gutenberglicence: Public domain (per item)year: —id: 56344citation: https://www.gutenberg.org/ebooks/56344characters: 200,001

record · JSON · record JSON

Related services and records

Services

  • Estate — measured countries, lanes and facts
  • Intel — live corroborated events
  • Legal — statutes, cases and citations
  • Encyclopedia — articles with inline sources
  • Space — launches, satellites and orbits
  • Search — federated search and reports
  • Pass — passport account and SSO
  • Corpora — read-only corpus origins
  • e01 — self-hosted corpora and tools

Text and metadata only; each target carries its own sources. Missing data is published as no-data, never estimated.