The Project Gutenberg eBook of Henley's Twentieth Century Formulas, Recipes and Processes This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Henley's Twentieth Century Formulas, Recipes and Processes Editor: Gardner Dexter Hiscox Release date: September 25, 2016 [eBook #53143] Most recently updated: October 23, 2024 Language: English Other information and formats: www.gutenberg.org/ebooks/53143 Credits: Produced by Brian Coe, RichardW, and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by University of California libraries, and by archive.org) *** START OF THE PROJECT GUTENBERG EBOOK HENLEY'S TWENTIETH CENTURY FORMULAS, RECIPES AND PROCESSES *** «HENLEY’S TWENTIETH CENTURY RECIPES, FORMULAS AND PROCESSES» CONTAINING TEN THOUSAND SELECTED HOUSEHOLD AND WORKSHOP FORMULAS, RECIPES, PROCESSES AND MONEY-SAVING METHODS FOR THE PRACTICAL USE OF MANUFACTURERS, MECHANICS, HOUSEKEEPERS AND HOME WORKERS EDITED BY GARDNER D. HISCOX, M.E. AUTHOR OF “MECHANICAL MOVEMENTS, POWERS AND DEVICES,” “COMPRESSED AIR,” “GAS, GASOLINE AND OI

source: Project Gutenberglicence: Public domain (per item)database: /home/dbs/gutenberg.dbmode: tablerecords: 544887 (max_rowid)citation: https://www.gutenberg.org/

The Project Gutenberg eBook of Henley's Twentieth Century Formulas, Recipes and Processes

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: Henley's Twentieth Century Formulas, Recipes and Processes

Editor: Gardner Dexter Hiscox

Release date: September 25, 2016 [eBook #53143]
Most recently updated: October 23, 2024

Language: English

Other information and formats: www.gutenberg.org/ebooks/53143

Credits: Produced by Brian Coe, RichardW, and the Online Distributed
Proofreading Team at http://www.pgdp.net (This file was
produced from images generously made available by University
of California libraries, and by archive.org)

*** START OF THE PROJECT GUTENBERG EBOOK HENLEY'S TWENTIETH CENTURY FORMULAS, RECIPES AND PROCESSES ***

«HENLEY’S TWENTIETH CENTURY RECIPES, FORMULAS AND PROCESSES»

CONTAINING TEN THOUSAND SELECTED HOUSEHOLD AND WORKSHOP FORMULAS,
RECIPES, PROCESSES AND MONEY-SAVING METHODS FOR THE PRACTICAL USE OF
MANUFACTURERS, MECHANICS, HOUSEKEEPERS AND HOME WORKERS

EDITED BY
GARDNER D. HISCOX, M.E.

AUTHOR OF “MECHANICAL MOVEMENTS, POWERS AND DEVICES,” “COMPRESSED
AIR,” “GAS, GASOLINE AND OIL ENGINES,” ETC., ETC.

[Illustration]

1914 EDITION, REVISED AND ENLARGED

NEW YORK
THE NORMAN W. HENLEY PUBLISHING COMPANY
132 NASSAU STREET
1914

COPYRIGHT, 1914 AND 1913, BY
THE NORMAN W. HENLEY PUBLISHING COMPANY

COPYRIGHT, 1912 AND 1907, BY
THE NORMAN W. HENLEY PUBLISHING COMPANY
Also, Entered at Stationers’ Hall Court, London, England

_All rights reserved_

THE TROW PRESS, NEW YORK

«PREFACE»

In compiling this book of formulas, recipes and processes, the Editor
has endeavored to meet the practical requirements of the home and
workshop—the mechanic, the manufacturer, the artisan, the housewife,
and the general home worker.

In addition to exercising the utmost care in selecting his materials
from competent sources, the Editor has also modified formulas which
were obviously ill adapted for his needs, but were valuable if altered.
Processes of questionable merit he has discarded. By adhering to this
plan the Editor trusts that he has succeeded in preparing a repository
of useful knowledge representing the experience of experts in every
branch of practical achievement. Much of the matter has been specially
translated for this work from foreign technological periodicals and
books. In this way the Editor has embodied much practical information
otherwise inaccessible to most English-speaking people.

Each recipe is to be regarded as a basis of experiment, to be modified
to suit the particular purpose in hand, or the peculiar conditions
which may affect the experimenter. Chemicals are not always of uniform
relative purity and strength; heat or cold may markedly influence the
result obtained, and lack of skill in the handling of utensils and
instruments may sometimes cause failure. Inasmuch as a particular
formula may not always be applicable, the Editor has thought it
advisable to give as many recipes as his space would allow under
each heading. In some instances a series of formulas is given which
apparently differ but slightly in their ingredients. This has been done
on the principle that one or more may be chosen for the purpose in hand.

Recognizing the fact that works of a similar character are not unknown,
the Editor has endeavored to present in these pages the most modern
methods and formulas. Naturally, old recipes and so-called trade
secrets which have proven their value by long use are also included,
particularly where no noteworthy advance has been made; but the primary
aim has been to modernize and bring the entire work up to the present
date.

THE EDITOR.

JANUARY, 1914.

«PARTIAL LIST OF AUTHORITIES CONSULTED»

Apothecary, The.
Berliner Drog. Zeitung.
Brass World.
British Journal of Photography.
Chemical News.
Chemiker Zeitung Repertorium.
Chemisch Technische Fabrikant.
Chemische Zeitung.
Chemist-Druggist.
Comptes Rendus.
Cooley’s Receipts.
Cosmos.
Dekorationsmaler, Der.
Deutsche Drog. Zeitung.
Deutsche Goldschmiede Zeitung.
Deutsche Handwerk.
Deutsche Maler Zeitung.
Deutsche Topfer und Ziefler Zeitung.
Dingler’s Polytechnic Journal.
Drogisten Zeitung.
Druggists’ Circular.
English Mechanic.
Farben Zeitung.
Gummi Zeitung.
Journal der Goldschmiedekunst.
Journal of Applied Microscopy.
Journal of the Franklin Institute.
Journal Society of Chemical Industry.
Journal Suisse d’Horlogerie.
Keramische Rundschau.
La Nature.
La Science en Famille.
La Vie Scientifique.
Lack und Farben Industrie.
Legierungen.
Le Genie Civil.
Le Praticien.
Leipziger Farber und Zeugdrucker Zeitung.
Maler Zeitung.
Metallarbeiter.
Mining and Scientific Press.
Neueste Erfindungen und Erfahrungen.
Nouvelles Scientifiques.
Oils, Colors, and Drysalteries.
Papier-Zeitung.
Parfumer, Der.
Pharmaceutische Zeitung.
Pharmaceutische Centralhalle.
Pharmaceutische Era.
Pharmaceutische Journal.
Pharmaceutische Journal Formulary.
Photo Times.
Polytech. Centralblatt.
Polyt. Notizblatt.
Popular Science News.
Pottery Gazette.
Practical Druggist.
Revue Chronometrique.
Revue de la Droguerie.
Revue des Produits Chimiques.
Revue Industrielle.
Science, Arts and Nature.
Science Pratique.
Seifensieder Zeitung, Der.
Seifenfabrikant, Der.
Spatula.
Stein der Weisen, Der.
Sudd. Apoth. Zeitung.
Technisches Centralblatt.
Technische Rundschau.
Uhland’s Technische Rundschau.
Verzinnen Verzinken Vernickeln, Das.
Werkmeister Zeitung.
Wiener Drogisten Zeitung.
Wiener Gewerbe Zeitung.
Zeitschrift für die Gesammte Kohlensaure Industrie.

{9}

«HENLEY’S BOOK OF RECIPES»

ABRASION REMEDY: See Cosmetics and Ointments.

ABSINTHE: See Wines and Liquors.

«Acid-Proofing»

«An Acid-Proof Table Top.»—

1.

Copper sulphate 1 part
Potassium chlorate 1 part
Water 8 parts

Boil until salts are dissolved.

2.

Aniline hydrochlorate 3 parts
Water 20 parts

Or, if more readily procurable:

Aniline 6 parts
Hydrochloric acid 9 parts
Water 50 parts

By the use of a brush two coats of solution No. 1 are applied while
hot; the second coat as soon as the first is dry. Then two coats of
solution No. 2, and the wood allowed to dry thoroughly. Later, a coat
of raw linseed oil is to be applied, using a cloth instead of a brush,
in order to get a thinner coat of the oil.

A writer in the _Journal of Applied Microscopy_ states that he has used
this method upon some old laboratory tables which had been finished in
the usual way, the wood having been filled oiled, and varnished. After
scraping off the varnish down to the wood, the solutions were applied,
and the result was very satisfactory.

After some experimentations the formula was modified without materially
affecting the cost, and apparently increasing the resistance of the
wood to the action of strong acids and alkalies. The modified formula
follows:

1.

Iron sulphate 4 parts
Copper sulphate 4 parts
Potassium permanganate 8 parts
Water, q. s. 100 parts

2.

Aniline 12 parts
Hydrochloric acid 18 parts
Water, q. s. 100 parts

Or:

Aniline hydrochlorate 15 parts
Water, q. s. 100 parts

Solution No. 2 has not been changed, except to arrange the parts per
hundred.

The method of application is the same, except that after solution No. 1
has dried the excess of the solution which has dried upon the surface
of the wood is thoroughly rubbed off before the application of solution
No. 2. The black color does not appear at once, but usually requires a
few hours before becoming ebony black. The linseed oil may be diluted
with turpentine without disadvantage, and after a few applications the
surface will take on a dull and not displeasing polish. The table tops
are easily cleaned by washing with water or suds after a course of work
is completed, and the application of another coat of oil puts them in
excellent order for another course of work. Strong acids or alkalies
when spilled, if soon wiped off, have scarcely a perceptible effect.

A slate or tile top is expensive not only in its original cost, but
also as a destroyer of glassware. Wood tops when painted, oiled, or
paraffined have objectionable features, the latter especially in warm
weather. Old table tops, after the paint or oil is scraped off down to
the wood, take the above finish nearly as well as the new wood.

«To Make Wood Acid- and Chlorine-Proof.»—Take 6 pounds of wood tar and
12 pounds rosin, and melt them together in an iron kettle, after which
stir in 8 pounds finely powdered brick dust. The damaged parts must be
cleaned perfectly and dried, whereupon they may be painted over with
the warm preparation or filled up and drawn off, leaving the film on
the inside.

«Protecting Cement Against Acid.»—A paint to protect cement against
acid is obtained by mixing pure asbestos, very finely powdered,
with a thick solution of {10} sodium silicate. The sodium silicate
must be as alkaline as possible. The asbestos is first rubbed with
a small quantity of the silicate, until a cake is obtained and then
kept in well-closed vessels. For use this cake is simply thinned with
a solution of the silicate, which furnishes a paint two or three
applications of which protect the walls of reservoirs, etc., against
any acid solid or liquid. This mass may also be employed for making a
coating of sandstone.

«To Make Corks Impermeable and Acid-Proof.»—Choose your corks
carefully. Then plunge them into a solution of gelatin or common glue,
15 parts, in 24 parts of glycerine and 500 parts of water, heated to
44° or 48° C. (112°–120° F.), and keep them there for several hours. On
removing the corks, which should be weighted down in the solution, dry
them in the shade until they are free from all surplus moisture. They
are now perfectly tight, retaining at the same time the greater portion
of their elasticity and suppleness. To render them acid-proof, they
should be treated with a mixture of vaseline, 2 parts, and paraffine
7 parts, heated to about 105° F. This second operation may be avoided
by adding to the gelatin solution a little ammonium dichromate and
afterwards exposing the corks to the light.

«Lining for Acid Receptacles.»—Plates are formed of 1 part of brown
slate, 2 of powdered glass, and 1 of Portland cement, the whole worked
up with silicate of soda, molded and dried. Make a cement composed of
ground slate and silicate of soda and smear the surface for the lining;
then, while it is still plastic, apply the plates prepared as above
described. Instead of these plates, slabs of glass or porcelain or
similar substances may be employed with the same cement.

ACACIA, MUCILAGE OF: See Adhesives under Mucilages.

ACID-PROOF GLASS: See Glass.

ACID-RESISTING PAINT: See Paint.

ACIDS, SOLDERING: See Solders.

ACID STAINS FROM THE SKIN, TO REMOVE: See Cleaning Preparations and
Methods.

ACID TEST FOR VINEGAR: See Vinegar.

«Adhesives»

«GLUES:»

«Manufacture of Glue.»—I.—The usual process of removing the phosphate
of lime from bones for glue-making purposes by means of dilute
hydrochloric acid has the disadvantage that the acid cannot be
regenerated. Attempts to use sulphurous acid instead have so far proved
unsuccessful, as, even with the large quantities used, the process
is very slow. According to a German invention this difficulty with
sulphurous acid can be avoided by using it in aqueous solution under
pressure. The solution of the lime goes on very rapidly, it is claimed,
and no troublesome precipitation of calcium sulphite takes place. Both
phosphate of lime and sulphurous acid are regenerated from the lyes by
simple distillation.

II.—Bones may be treated with successive quantities of combined
sulphurous acid and water, from which the heat of combination has been
previously dissipated, the solution being removed after each treatment,
before the bone salts dissolved therein precipitate, and before the
temperature rises above 74° F.—U. S. Pat. 783,784.

III.—A patent relating to the process for treating animal sinews,
preparatory for the glue factory, has been granted to Florsheim,
Chicago, and consists in immersing animal sinews successively in
petroleum or benzine to remove the outer fleshy animal skin; in
a hardening or preserving bath, as boric acid, or alum or copper
sulphate; and in an alkaline bath to remove fatty matter from the
fibrous part of the sinews. The sinews are afterwards tanned and
disintegrated.

«Test for Glue.»—The more water the glue takes up, swelling it, the
better it is. Four ounces of the glue to be examined are soaked for
about 12 hours in a cool place in 4 pounds of cold water. If the glue
has dissolved after this time, it is of bad quality and of little
value; but if it is coherent, gelatinous, and weighing double, it is
good; if it weighs up to 16 ounces, it is very good; if as much as 20
ounces, it may be called excellent.

«To Prevent Glue from Cracking.»—To prevent glue from cracking, which
frequently occurs when glued articles are {11} exposed to the heat of a
stove, a little chloride of potassium is added. This prevents the glue
from becoming dry enough to crack. Glue thus treated will adhere to
glass, metals, etc., and may also be used for pasting on labels.

«Preventing the Putrefaction of Strong Glues.»—The fatty matter always
existing in small quantity in sheets of ordinary glue affects the
adhesive properties and facilitates the development of bacteria, and
consequently putrefaction and decomposition. These inconveniences are
remedied by adding a small quantity of caustic soda to the dissolved
glue. The soda prevents decomposition absolutely; with the fatty matter
it forms a hard soap which renders it harmless.

«Liquid Glues.»—

I.—Glue 3 ounces
Gelatin 3 ounces
Acetic acid 4 ounces
Water 2 ounces
Alum 30 grains

Heat together for 6 hours, skim, and add:

II.—Alcohol 1 fluid ounce
Brown glue, No. 2. 2 pounds
Sodium carbonate 11 ounces
Water 3 1⁠/⁠2 pints
Oil of clove 160 minims

Dissolve the soda in the water, pour the solution over the dry glue,
let stand over night or till thoroughly soaked and swelled, then heat
carefully on a water bath until dissolved. When nearly cold stir in the
oil of cloves.

By using white glue, a finer article, fit for fancy work, may be made.

III.—Dissolve by heating 60 parts of borax in 420 parts of water,
add 480 parts dextrin (pale yellow) and 50 parts of glucose and heat
carefully with continued stirring, to complete solution; replace the
evaporated water and pour through flannel.

The glue made in this way remains clear quite a long time, and
possesses great adhesive power; it also dries very quickly, but upon
careless and extended heating above 90° C. (194° F.), it is apt to turn
brown and brittle.

IV.—Pour 50 parts of warm (not hot) water over 50 parts of Cologne glue
and allow to soak over night. Next day the swelled glue is dissolved
with moderate heat, and if still too thick, a little more water is
added. When this is done, add from 2 1⁠/⁠2 to 3 parts of crude nitric
acid, stir well, and fill the liquid glue in well-corked bottles. This
is a good liquid steam glue.

V.—Soak 1 pound of good glue in a quart of water for a few hours, then
melt the glue by heating it, together with the unabsorbed water, then
stir in 1⁠/⁠4 pound dry white lead, and when that is well mixed pour in
4 fluidounces of alcohol and continue the boiling 5 minutes longer.

VI.—Soak 1 pound of good glue in 1 1⁠/⁠2 pints of cold water for
5 hours, then add 3 ounces of zinc sulphate and 2 fluidounces of
hydrochloric acid, and keep the mixture heated for 10 or 12 hours at
175° to 190° F. The glue remains liquid and may be used for sticking a
variety of materials.

VII.—A very inexpensive liquid glue may be prepared by first soaking
and then dissolving gelatin in twice its own weight of water at a very
gentle heat; then add glacial acetic acid in weight equal to the weight
of the dry gelatin. It should be remembered, however, that all acid
glues are not generally applicable.

VIII.—Glue 200 parts
Dilute acetic acid 400 parts

Dissolve by the aid of heat and add:

Alcohol 25 parts
Alum 5 parts

IX.—Glue 5 parts
Calcium chloride 1 part
Water 1 part

X.—Sugar of lead 1 1⁠/⁠2 drachms
Alum 1 1⁠/⁠2 drachms
Gum arabic 2 1⁠/⁠2 drachms
Wheat flour 1 av. lb.
Water, q. s.

Dissolve the gum in 2 quarts of warm water; when cold mix in the flour,
and add the sugar of lead and alum dissolved in water; heat the whole
over a slow fire until it shows signs of ebullition. Let it cool, and
add enough gum water to bring it to the proper consistence.

XI.—Dilute 1 part of official phosphoric acid with 2 parts of water and
neutralize the solution with carbonate of ammonium. Add to the liquid
an equal quantity of water, warm it on a water bath, and dissolve in it
sufficient glue to form a thick syrupy liquid. Keep in well-stoppered
bottles.

XII.—Dissolve 3 parts of glue in small pieces in 12 to 15 of saccharate
of lime. By heating, the glue dissolves rapidly and remains liquid,
when cold, without loss of adhesive power. Any desirable consistence
can be secured by varying the amount of saccharate of lime. Thick
glue retains its muddy color, while a thin solution becomes clear on
standing.

The saccharate of lime is prepared by {12} dissolving 1 part of sugar
in 3 parts of water, and after adding 1⁠/⁠4 part of the weight of the
sugar of slaked lime, heating the whole from 149° to 185° F., allowing
it to macerate for several days, shaking it frequently. The solution,
which has the properties of mucilage, is then decanted from the
sediment.

XIII.—In a solution of borax in water soak a good quantity of glue
until it has thoroughly imbibed the liquid. Pour off the surplus
solution and then put on the water bath and melt the glue. Cool down
until the glue begins to set, then add, drop by drop, with agitation,
enough acetic acid to check the tendency to solidification. If, after
becoming quite cold, there is still a tendency to solidification, add a
few drops more of the acid. The liquid should be of the consistence of
ordinary mucilage at all times.

XIV.—Gelatin 100 parts
Cabinetmakers’ glue 100 parts
Alcohol 25 parts
Alum 2 parts
Acetic acid, 20 per cent 800 parts

Soak the gelatin and glue with the acetic acid and heat on a water bath
until fluid; then add the alum and alcohol.

XV.—Glue 10 parts
Water 15 parts
Sodium salicylate 1 part

XVI.—Soak 5 parts of Cologne glue in an aqueous calcium chloride
solution (1:4) and heat on the water bath until dissolved, replacing
the evaporating water; or slack 100 parts of lime with 150 parts of hot
water, dissolve 60 parts of sugar in 180 parts of water, and add 15
parts of the slacked lime to the solution, heating the whole to 75° C.
(167° F.). Place aside for a few days, shaking from time to time. In
the clear sugar-lime solution collected by decanting soak 60 parts of
glue and assist the solution by moderate heating.

XVII.—Molasses, 100 parts, dissolved in 300 parts of water, 25 parts
of quicklime (slaked to powder), being then stirred in and the
mixture heated to 167° F. on a water bath, with frequent stirrings.
After settling for a few days a large portion of the lime will have
dissolved, and the clear, white, thick solution, when decanted, behaves
like rubber solution and makes a highly adherent coating.

XVIII.—Dissolve bone glue, 250 parts, by heating in 1,000 parts of
water, and add to the solution barium peroxide 10 parts, sulphuric acid
(66° B.) 5 parts, and water 15 parts. Heat for 48 hours on the water
bath to 80° C. (176° F.). Thus a syrupy liquid is obtained, which is
allowed to settle and is then decanted. This glue has no unpleasant
odor, and does not mold.

XIX.—A glue possessing the adhesive qualities of ordinary joiners’
glue, but constituting a pale yellow liquid which is ready for use
without requiring heating and possesses great resistance to dampness,
is produced by treating dry casein with a diluted borax solution or
with enough ammonia solution to cause a faintly alkaline reaction. The
preparation may be employed alone or mixed with liquid starch in any
proportion.

«Glue for Celluloid.»—I.—Two parts shellac, 3 parts spirits of camphor,
and 4 parts strong alcohol dissolved in a warm place, give an excellent
gluing agent to fix wood, tin, and other bodies to celluloid. The glue
must be kept well corked up.

II.—A collodion solution may be used, or an alcoholic solution of fine
celluloid shavings.

«Glue to Form Paper Pads.»—

I.—Glue 3 1⁠/⁠2 ounces
Glycerine 8 ounces
Water, a sufficient quantity.

Pour upon the glue more than enough water to cover it and let stand for
several hours, then decant the greater portion of the water; apply heat
until the glue is dissolved, and add the glycerin. If the mixture is
too thick, add more water.

II.—Glue 6 ounces
Alum 30 grains
Acetic acid 1⁠/⁠2 ounce
Alcohol 1 1⁠/⁠2 ounces
Water 6 1⁠/⁠2 ounces

Mix all but the alcohol, digest on a water bath till the glue is
dissolved, allow to cool and add the alcohol.

III.—Glue 5 ounces
Water 1 ounce
Calcium chloride 1 ounce

Dissolve the calcium chloride in the water, add the glue, macerate
until it is thoroughly softened, and then heat until completely
dissolved.

IV.—Glue 20 ounces
Glycerine 5 ounces
Syrupy glucose 1 ounce
Tannin 50 grains

Cover the glue with cold water, and let stand over night. In the
morning pour off superfluous water, throw the glue on muslin, and
manipulate so as to get rid of as much moisture as possible, then put
in a water bath and melt. Add the {13} glycerine and syrup, and stir
well in. Finally, dissolve the tannin in the smallest quantity of water
possible and add.

This mixture must be used hot.

V.—Glue 15 ounces
Glycerine 5 ounces
Linseed oil 2 ounces
Sugar 1 ounce

Soak the glue as before, melt, add the sugar and glycerine, continuing
the heat, and finally add the oil gradually under constant stirring.

This must be used hot.

«Glue for Tablets.»—

I.—Glue 3 1⁠/⁠2 ounces
Glycerine 8 ounces
Water, a sufficient quantity.

Pour upon the glue more than enough water to cover it and let stand for
several hours, then decant the greater portion of the water; apply heat
until the glue is dissolved, and add the glycerine. If the mixture is
too thick, add more water.

II.—Glue 6 ounces
Alum 30 grains
Acetic acid 1⁠/⁠2 ounce
Alcohol 1 1⁠/⁠2 ounces
Water 6 1⁠/⁠2 ounces

Mix all but the alcohol, digest on a water bath till the glue is
dissolved, allow to cool and add the alcohol.

III.—Glue 5 ounces
Water 1 ounce
Calcium chloride 1 ounce

Dissolve the calcium chloride in the water, add the glue, macerate
until it is thoroughly softened, and then apply heat until completely
dissolved.

IV.—Glue, 1 pound; glycerine, 4 ounces; glucose syrup, 2
tablespoonfuls; tannin, 1⁠/⁠10 ounce. Use warm, and give an hour to dry
and set on the pads. This can be colored with any aniline dye.

«Marine Glue.»—Marine glue is a product consisting of shellac and
caoutchouc, which is mixed differently according to the use for which
it is required. The quantity of benzol used as solvent governs the
hardness or softness of the glue.

I.—One part Pará caoutchouc is dissolved in 12 parts benzol; 20
parts powdered shellac are added to the solution, and the mixture is
carefully heated.

II.—Stronger glue is obtained by dissolving 10 parts good crude
caoutchouc in 120 parts benzine or naphtha which solution is poured
slowly and in a fine stream into 20 parts asphaltum melted in a kettle,
stirring constantly and heating. Pour the finished glue, after the
solvent has almost evaporated and the mass has become quite uniform,
into flat molds, in which it solidifies into very hard tablets of dark
brown or black color. For use, these glue tablets are first soaked in
boiling water and then heated over a free flame until the marine glue
has become thinly liquid. The pieces to be glued are also warmed and a
very durable union is obtained.

III.—Cut caoutchouc into small pieces and dissolve in coal naphtha by
heat and agitation. Add to this solution powdered shellac, and heat
the whole, constantly stirring until combination takes place, then pour
it on metal plates to form sheets. When used it must be heated to 248°
F., and applied with a brush.

«Water-Proof Glues.»—I.—The glue is put in water till it is soft, and
subsequently melted in linseed oil at moderate heat. This glue is
affected neither by water nor by vapors.

II.—Dissolve a small quantity of sandarac and mastic in a little
alcohol, and add a little turpentine. The solution is boiled in a
kettle over the fire, and an equal quantity of a strong hot solution of
glue and isinglass is added. Then filter through a cloth while hot.

III.—Water-proof glue may also be produced by the simple addition of
bichromate of potassium to the liquid glue solution, and subsequent
exposure to the air.

IV.—Mix glue as usual, and then add linseed oil in the proportion of
1 part oil to 8 parts glue. If it is desired that the mixture remain
liquid, 1⁠/⁠2 ounce of nitric acid should be added to every pound of
glue. This will also prevent the glue from souring.

V.—In 1,000 parts of rectified alcohol dissolve 60 parts of sandarac
and as much mastic whereupon add 60 parts of white oil of turpentine.
Next, prepare a rather strong glue solution and add about the like
quantity of isinglass, heating the solution until it commences to boil;
then slowly add the hot glue solution till a thin paste forms, which
can still be filtered through a cloth. Heat the solution before use and
employ like ordinary glue. A connection effected with this glue is not
dissolved by cold water and even resists hot water for a long time.

VI.—Soak 1,000 parts of Cologne glue in cold water for 12 hours and in
another vessel for the same length of time 150 parts of isinglass in a
mixture of lamp spirit and water. Then dissolve both masses together on
the water bath in a suitable vessel, thinning, if necessary, with some
hot water. Next add 100 {14} parts of linseed oil varnish and filter
hot through linen.

VII.—Ordinary glue is kept in water until it swells up without losing
its shape. Thus softened it is placed in an iron crucible without
adding water; then add linseed oil according to the quantity of the
glue and leave this mixture to boil over a slow fire until a gelatinous
mass results. Such glue unites materials in a very durable manner. It
adheres firmly and hardens quickly. Its chief advantage, however,
consists in that it neither absorbs water nor allows it to pass
through, whereby the connecting places are often destroyed. A little
borax will prevent putrefaction.

VIII.—Bichromate of potassium 40 parts (by weight); gelatin glue, 55
parts; alum, 5 parts. Dissolve the glue in a little water and add the
bichromate of potassium and the alum.

IX.—This preparation permits an absolutely permanent gluing of pieces
of cardboard, even when they are moistened by water. Melt together
equal parts of good pitch and gutta-percha; of this take 9 parts, and
add to it 3 parts of boiled linseed oil and 1 1⁠/⁠2 parts of litharge.
Place this over the fire and stir it till all the ingredients are
intimately mixed. The mixture may be diluted with a little benzine or
oil of turpentine, and must be warm when used.

«Glue to Fasten Linoleum on Iron Stairs.»—I.—Use a mixture of glue,
isinglass, and dextrin which, dissolved in water and heated, is given
an admixture of turpentine. The strips pasted down must be weighted
with boards and brick on top until the adhesive agent has hardened.

II.—Soak 3 parts of glue in 8 parts water, add 1⁠/⁠2 part hydrochloric
acid and 3⁠/⁠4 part zinc vitriol and let this mixture boil several
hours. Coat the floor and the back of the linoleum with this. Press the
linoleum down uniformly and firmly and weight it for some time.

«Glue for Attaching Gloss to Precious Metals.»—Sandarac varnish, 15
parts; marine glue, 5 parts; drying oil, 5 parts; white lead, 5 parts;
Spanish white, 5 parts; turpentine, 5 parts. Triturate all to form a
rather homogeneous paste. This glue becomes very hard and resisting.

«Elastic Glue.»—Although elastic glue is less durable than rubber,
and will not stand much heat, yet it is cheaper than rubber, and is
not, like rubber affected by oil colors. Hence it is largely used for
printing rollers and stamps. For stamps, good glue is soaked for 24
hours in soft water. The water is poured off, and the swollen glue is
melted and mixed with glycerine and a little salicylic acid and cast
into molds. The durability is increased by painting the mass with a
solution of tannin, or, better, of bichromate of potassium. Printing
rollers require greater firmness and elasticity. The mass for them
once consisted solely of glue and vinegar, and their manufacture was
very difficult. The use of glycerine has remedied this, and gives
great elasticity without adhesiveness, and has removed the liability
of moldiness. Swollen glue, which has been superficially dried, is
fused with glycerine and cast into oil molds. Similar mixtures are
used for casting plaster ornaments, etc., and give very sharp casts.
A mass consisting of glue and glycerine is poured over the model in a
box. When the mold is removed, it is painted with plaster outside and
with boiled oil inside, and can then be used many times for making
reproductions of the model.

«Glue for Paper and Metal.»—A glue which will keep well and adhere
tightly is obtained by diluting 1,000 parts by weight of potato starch
in 1,200 parts by weight of water and adding 50 parts by weight of
pure nitric acid. The mixture is kept in a hot place for 48 hours,
taking care to stir frequently. It is afterwards boiled to a thick and
transparent consistency, diluted with water if there is occasion, and
then there are added in the form of a screened powder, 2 parts of sal
ammoniac and 1 part of sulphur flowers.

«Glue for Attaching Cloth Strips to Iron.»—Soak 500 parts of Cologne
glue in the evening with clean cold water in a clean vessel; in the
morning pour off the water, place the softened glue without admixture
of water into a clean copper or enamel receptacle, which is put on a
moderate low fire (charcoal or steam apparatus). During the dissolution
the mass must be continually stirred with a wooden trowel or spatula.
If the glue is too thick, it is thinned with diluted spirit, but not
with water. As soon as the glue has reached the boiling point, about
50 parts of linseed oil varnish (boiled oil) is added to the mass with
constant stirring. When the latter has been stirred up well, add 50
parts of powdered colophony and shake it into the mass with stirring,
subsequently removing the glue from the fire. In order to increase the
binding qualities and to guard against moisture, it is well still to
add about 50 parts of isinglass, which has been previously cut {15}
into narrow strips and placed, well beaten, in a vessel, into which
enough spirit of wine has been poured to cover all. When dissolved, the
last-named mass is added to the boiling glue with constant stirring.
The adhesive agent is now ready for use and is employed hot, it
being advisable to warm the iron also. Apply glue only to a surface
equivalent to a single strip at a time. The strips are pressed down
with a stiff brush or a wad of cloth.

«Glue for Leather or Cardboard.»—To attach leather to cardboard
dissolve good glue (softened by spelling in water) with a little
turpentine and enough water in an ordinary glue pot, and then having
made a thick paste with starch in the proportion of 2 parts by weight,
of starch powder for every 1 part, by weight, of dry glue, mix the
compounds and allow the mixture to become cold before application to
the cardboard.

«For Wood, Glass, Cardboard, and all Articles of a Metallic or Mineral
Character.»—Take boiled linseed oil 20 parts, Flemish glue 20 parts,
hydrated lime 15 parts, powdered turpentine 5 parts, alum 5 parts
acetic acid 5 parts. Dissolve the glue with the acetic acid, add the
alum, then the hydrated lime, and finally the turpentine and the boiled
linseed oil. Triturate all well until it forms a homogeneous paste and
keep in well-closed flasks. Use like any other glue.

«Glue for Uniting Metals with Fabrics.»—Cologne glue of good quality
is soaked and boiled down to the consistency of that used by
cabinetmakers. Then add, with constant stirring, sifted wood ashes
until a moderately thick, homogeneous mass results. Use hot and press
the pieces well together during the drying. For tinfoil, about 2 per
cent of boracic acid should be added instead of the wood ashes.

«Glue or Paste for Making Paper Boxes.»—

Chloral hydrate 5 parts
Gelatin, white 8 parts
Gum arabic 2 parts
Boiling water 30 parts

Mix the chloral, gelatin, and gum arabic in a porcelain container, pour
the boiling water over the mixture and let stand for 1 day, giving it
a vigorous stirring several times during the day. In cold weather this
is apt to get hard and stiff, but this may be obviated by standing the
container in warm water for a few minutes. This paste adheres to any
surface whatever.

«Natural Glue for Cementing Porcelain, Crystal Glass, etc.»—The large
shell snails which are found in vineyards have at the extremity of
their body a small, whitish bladder filled with a substance of greasy
and gelatinous aspect. If this substance extracted from the bladder
is applied on the fragments of porcelain or any body whatever, which
are juxtaposed by being made to touch at all parts, they acquire such
adhesion that if one strives to separate them by a blow, they are
more liable to break at another place than the cemented seam. It is
necessary to give this glue sufficient time to dry perfectly, so as to
permit it to acquire the highest degree of strength and tenacity.

«Belt Glue.»—A glue for belts can be prepared as follows: Soak 50
parts of gelatin in water, pour off the excess of water, and heat on
the water bath. With good stirring add, first, 5 parts, by weight, of
glycerine, then 10 parts, by weight, of turpentine, and 5 parts, by
weight, of linseed oil varnish and thin with water as required. The
ends of the belts to be glued are cut off obliquely and warmed; then
the hot glue is applied, and the united parts are subjected to strong
pressure, allowing them to dry thus for 24 hours before the belts are
used.

«Chromium Glue for Wood, Paper, and Cloth.»—I.—(_a_) One-half pound
strong glue (any glue if color is immaterial, white fish glue
otherwise); soak 12 hours in 12 fluidounces of cold water. (_b_)
One-quarter pound gelatin; soak 2 hours in 12 fluidounces cold water.
(_c_) Two ounces bichromate of potassium dissolved in 8 fluidounces
boiling water. Dissolve (_a_) after soaking, in a glue pot, and add
(_b_). After (_a_) and (_b_) are mixed and dissolved, stir in (_c_).
This glue is exceedingly strong, and if the article cemented be exposed
to strong sunlight for 1 hour, the glue becomes perfectly waterproof.
Of course, it is understood that the exposure to sunlight is to be made
after the glue is thoroughly dry. The one objectionable feature of this
cement is its color, which is a yellow-brown. By substituting chrome
alum in place of the bichromate, an olive color is obtained.

II.—Use a moderately strong gelatin solution (containing 5 to 10
per cent of dry gelatin), to which about 1 part of acid chromate of
potassium in solution is added to every 5 parts of gelatin. This
mixture has the property of becoming insoluble by water through the
action of sunlight under partial reduction of the chromic acid. {16}

«Fireproof Glue.»—

Raw linseed oil 8 parts
Glue or gelatin 1 part
Quicklime 2 parts

Soak the glue or gelatin in the oil for 10 to 12 hours, and then melt
it by gently heating the oil, and when perfectly fluid stir in the
quicklime until the whole mass is homogeneous, then spread out in
layers to dry gradually, out of the sun’s rays. For use, reheat the
glue in a glue pot in the ordinary way of melting glue.

«CEMENTS.»

Under this heading will be found only cements for causing one substance
to adhere to another. Cements used primarily as fillers, such as dental
cements, will be found under Cements, Putties, etc.

«Cutlers’ Cements for Fixing Knife Blades into Handles.»—

I.—Rosin 4 pounds
Beeswax 1 pound
Plaster of Paris or brickdust 1 pound

II.—Pitch 5 pounds
Wood ashes 1 pound
Tallow 1 pound

III.—Rosin, 12; sulphur flowers, 3; iron filings, 5. Melt together,
fill the handle while hot, and insert the instrument.

IV.—Plaster of Paris is ordinarily used for fastening loose handles.
It is made into a moderately thick paste with water run into the hole
in the head of the pestle, the handle inserted and held in place till
the cement hardens. Some add sand to the paste, and claim to get better
results.

V.—Boil together 1 part of caustic soda, 3 parts of rosin, and 5 parts
of water till homogeneous and add 4 parts of plaster of Paris. The
paste sets in half an hour and is but little affected by water.

VI.—Equal quantities of gutta percha and shellac are melted together
and well stirred. This is best done in an iron capsule placed on a
sandbath and heated over a gas furnace or on the top of a stove. The
combination possesses both hardness and toughness, qualities that make
it particularly desirable in mending mortars and pestles. In using, the
articles to be cemented should be warmed to about the melting point of
the mixture and retained in proper position until cool, when they are
ready for use.

VII.—Rosin 600 parts by weight
Sulphur 150 parts by weight
Iron filings 250 parts by weight

Pour the mixture, hot, into the opening of the heated handle and shove
in the knife likewise heated.

VIII.—Melt sufficient black rosin, and incorporate thoroughly with it
one-fifth its weight of very fine silver sand. Make the pestle hot,
pour in a little of the mixture, then force the handle well home, and
set aside for a day before using.

IX.—Make a smooth, moderately soft paste with litharge and glycerine;
fill the hole in the pestle with the cement, and firmly press the
handle in place, keeping it under pressure for three or four days.

«Cements for Stone.»—I.—An excellent cement for broken marble consists
of 4 parts of gypsum and 1 part of finely powdered gum arabic. Mix
intimately. Then with a cold solution of borax make into a mortarlike
mass. Smear on each face of the parts to be joined, and fasten the bits
of marble together. In the course of a few days the cement becomes
very hard and holds very tenaciously. The object mended should not be
touched for several days. In mending colored marbles the cement may be
given the hue of the marble by adding the color to the borax solution.

II.—A cement which dries instantaneously, qualifying it for all sorts
of repairing and only presenting the disadvantage of having to be
freshly prepared each time, notwithstanding any subsequent heating, may
be made as follows: In a metal vessel or iron spoon melt 4 to 5 parts
of rosin (or preferably mastic) and 1 part of beeswax. This mixture
must be applied rapidly, it being of advantage slightly to heat the
surfaces to be united, which naturally must have been previously well
cleaned.

III.—Slaked lime, 10 parts; chalk, 15 parts; kaolin, 5 parts; mix, and
immediately before use stir with a corresponding amount of potash water
glass.

IV.—Cement on Marble Slabs.—The whole marble slab is thoroughly warmed
and laid face down upon a neatly cleaned planing bench upon which a
woolen cloth is spread so as not to injure the polish of the slab. Next
apply to the slab very hot, weak glue and quickly sift hot plaster of
Paris on the glue in a thin even layer, stirring the plaster rapidly
into the applied glue by means of a strong spatula, so that a uniform
glue-plaster coating is formed on the warm slab. Before this has time
to harden tip the respective piece of furniture on the slab. The frame,
likewise warmed, will adhere very firmly to the slab after two days.
Besides, this process has the advantage of great cleanliness. {17}

V.—The following is a recipe used by marble workers, and which probably
can be used to advantage: Flour of sulphur, 1 part; hydrochlorate of
ammonia, 2 parts; iron filings, 16 parts. The above substances must
be reduced to a powder, and securely preserved in closely stoppered
vessels. When the cement is to be employed, take 20 parts very fine
iron filings and 1 part of the above powder; mix them together with
enough water to form a manageable paste. This paste solidifies in 20
days and becomes as hard as iron. A recipe for another cement useful
for joining small pieces of marble or alabaster is as follows: Add
1⁠/⁠2 pint of vinegar to 1⁠/⁠2 pint skimmed milk; mix the curd with the
whites of 5 eggs, well beaten, and sufficient powdered quicklime sifted
in with constant stirring so as to form a paste. It resists water and a
moderate degree of heat.

VI.—Cement for Iron and Marble.—For fastening iron to marble or stone a
good cement is made as follows: Thirty parts plaster of Paris, 10 parts
iron filings, 1⁠/⁠2 part sal ammoniac mixed with vinegar to a fluid
paste fresh for use.

«Cement for Sandstones.»—One part sulphur and 1 part rosin are melted
separately; the melted masses are mixed and 3 parts litharge and 2
parts ground glass stirred in. The latter ingredients must be perfectly
dry, and have been well pulverized and mixed previously.

Equally good cement is obtained by melting together 1 part pitch and
1⁠/⁠10 part wax, and mixing with 2 parts brickdust.

The stones to be cemented, or between the joints of which the putty
is to be poured, must be perfectly dry. If practicable, they should
be warmed a little, and the surfaces to which the putty is to adhere
painted with oil varnish once or twice. The above two formulæ are of
especial value in case the stones are very much exposed to the heat
of the sun in summer, as well as to cold, rain, and snow in winter.
Experience has shown that in these instances the above-mentioned
cements give better satisfaction than the other brands of cement.

«Cements for Attaching Objects to Glass.»—

Rosin 1 part
Yellow wax 2 parts

Melt together.

«To Attach Copper to Glass.»—Boil 1 part of caustic soda and 3 parts of
colophony in 5 parts of water and mix with the like quantity of plaster
of Paris. This cement is not attacked by water, heat, and petroleum.
If, in place of the plaster of Paris, zinc white, white lead, or slaked
lime is used, the cement hardens more slowly.

«To Fasten Brass upon Glass.»—Boil together 1 part of caustic soda, 3
parts of rosin, 3 parts of gypsum, and 5 parts of water. The cement
made in this way hardens in about half an hour, hence it must
be applied quickly. During the preparation it should be stirred
constantly. All the ingredients used must be in a finely powdered state.

«Uniting Glass with Horn.»—(1) A solution of 2 parts of gelatin in
20 parts water is evaporated up to one-sixth of its volume and 1⁠/⁠3
mastic dissolved in 1⁠/⁠2 spirit added and some zinc white stirred in.
The putty is applied warm; it dries easily and can be kept a long time.
(2) Mix gold size with the equal volume of water glass.

«To Cement Glass to Iron.»—

I.—Rosin 5 ounces
Yellow wax 1 ounce
Venetian red 1 ounce

Melt the wax and rosin on a water bath and add, under constant
stirring, the Venetian red previously well dried. Stir until nearly
cool, so as to prevent the Venetian red from settling to the bottom.

II.—Portland cement 2 ounces
Prepared chalk 1 ounce
Fine sand 1 ounce
Solution of sodium silicate
enough to form a semi-liquid
paste.
III.—Litharge 2 parts
White lead 1 part

Work into a pasty condition by using 3 parts boiled linseed oil, 1 part
copal varnish.

«Celluloid Cements.»—I.—To mend broken draughting triangles and other
celluloid articles, use 3 parts alcohol and 4 parts ether mixed
together and applied to the fracture with a brush until the edges
become warm. The edges are then stuck together, and left to dry for at
least 24 hours.

II.—Camphor, 1 part; alcohol, 4 parts. Dissolve and add equal quantity
(by weight) of shellac to this solution.

III.—If firmness is desired in putting celluloid on wood, tin, etc.,
the following gluing agent is recommended, viz.: A compound of 2 parts
shellac, 3 parts spirit of camphor, and 4 parts strong alcohol. {18}

IV.—Shellac 2 ounces
Spirits of camphor 2 ounces
Alcohol, 90 per cent 6 to 8 ounces

V.—Make a moderately strong glue or solution of gelatin. In a dark
place or a dark room mix with the above a small amount of concentrated
solution of potassium dichromate. Coat the back of the label, which
must be clean, with a thin layer of the mixture. Strongly press the
label against the bottle and keep the two in close contact by tying
with twine or otherwise. Expose to sunlight for some hours; this causes
the cement to be insoluble even in hot water.

VI.—Lime av. oz. 1
White of egg av. oz. 2 1⁠/⁠2
Plaster of Paris av. oz. 5 1⁠/⁠2
Water fl. oz. 1

Reduce the lime to a fine powder; mix it with the white of egg by
trituration, forming a uniform paste. Dilute with water, rapidly
incorporate the plaster of Paris, and use the cement immediately. The
surfaces to be cemented must first be moistened with water so that the
cement will readily adhere. The pieces must be firmly pressed together
and kept in this position for about 12 hours.

«Cementing Celluloid and Hard-Rubber Articles.»—I.—Celluloid articles
can be mended by making a mixture composed of 3 parts of alcohol and 4
parts of ether. This mixture should be kept in a well-corked bottle,
and when celluloid articles are to be mended, the broken surfaces are
painted over with the alcohol and ether mixture until the surfaces
soften: then press together and bind and allow to dry for at least 24
hours.

II.—Dissolve 1 part of gum camphor in 4 parts of alcohol; dissolve an
equal weight of shellac in such strong camphor solution. The cement
is applied warm and the parts united must not be disturbed until the
cement is hard. Hard-rubber articles are never mended to form a strong
joint.

III.—Melt together equal parts of gutta percha and real asphaltum. The
cement is applied hot, and the broken surfaces pressed together and
held in place while cooling.

«Sign-Letter Cements.»—

I.—Copal varnish 15 parts
Drying oil 5 parts
Turpentine (spirits) 3 parts
Oil of turpentine 2 parts
Liquefied glue 5 parts

Melt all together on a water bath until well mixed, and then add 10
parts slaked lime.

II.—Mix 100 parts finely powdered white litharge with 50 parts dry
white lead, knead together 3 parts linseed oil varnish and 1 part copal
varnish into a firm dough. Coat the side to be attached with this,
removing the superfluous cement. It will dry quickly and become very
hard.

III.—Copal varnish 15 parts
Linseed-oil varnish 5 parts
Raw turpentine 3 parts
Oil of turpentine 2 parts
Carpenters’ glue, dissolved in water 5 parts
Precipitated chalk 10 parts

IV.—Mastic gum 1 part
Litharge, lead 2 parts
White lead 1 part
Linseed oil 3 parts

Melt together to a homogeneous mass. Apply hot. To make a thorough and
reliable job, the letters should be heated to at least the temperature
of the cement.

«To Fix Gold Letters, etc., upon Glass.»—I.—The glass must be entirely
clean and polished, and the medium is prepared in the following manner:
One ounce fish glue or isinglass is dissolved in water so that the
latter covers the glue. When this is dissolved a quart of rectified
spirit of wine is added, and enough water is poured in to make up
one-quarter the whole. The substance must be kept well corked.

II.—Take 1⁠/⁠2 quart of the best rum and 1⁠/⁠4 ounce fish glue, which
is dissolved in the former at a moderate degree of heat. Then add 1⁠/⁠2
quart distilled water, and filter through a piece of old linen. The
glass is laid upon a perfectly level table and is covered with this
substance to the thickness of 1⁠/⁠8 inch, using a clean brush. Seize
the gold leaf with a pointed object and place it smoothly upon the
prepared mass, and it will be attracted by the glass at once. After 5
minutes hold the glass slightly slanting so that the superfluous mass
can run off, and leave the plate in this position for 24 hours, when
it will be perfectly dry. Now trace the letters or the design on a
piece of paper, and perforate the lines with a thick needle, making
the holes 1⁠/⁠16 inch apart. Then place the perforated paper upon the
surface of the glass, and stamp the tracery on with powdered chalk.
The paper pattern is then carefully removed, and the accurate design
will remain upon the gold. The outlines are now filled out with an oily
gold mass, mixed with a little chrome orange and diluted with boiled
oil or turpentine. When all is dry the superfluous gold is washed off
{19} with water by means of a common rag. The back of the glass is then
painted with a suitable color.

«Attaching Enamel Letters to Glass.»—To affix enamel letters to glass,
first clean the surface of the glass perfectly, leaving no grease or
sticky substance of any kind adhering to the surface. Then with a piece
of soap sketch the outlines of the design. Make the proper division
of the guide lines, and strike off accurately the position each letter
is to occupy. Then to the back of the letters apply a cement made as
follows: White lead ground in oil, 2 parts; dry white lead, 3 parts.
Mix to a soft putty consistency with good copal varnish.

With a small knife or spatula apply the cement to the back of the
letters, observing especial care in getting the mixture well and
uniformly laid around the inside edges of the letter. In attaching
the letters to the glass make sure to expel the air from beneath the
characters, and to do this, work them up and down and sidewise. If the
weather be at all warm, support the letters while drying by pressing
tiny beads of sealing wax against the glass, close to the under side
or bottom of the letters. With a putty knife, keenly sharpened on one
edge, next remove all the surplus cement. Give the letters a hard, firm
pressure against the glass around all edges to securely guard against
the disruptive attacks of moisture.

The seepage of moisture beneath the surface of the letters is the main
cause of their early detachment from the glass.

The removal of the letters from the glass may be effected by applying
turpentine to the top of the characters, allowing it to soak down and
through the cement. Oxalic acid applied in the same way will usually
slick the letters off in a trice.

«Cement for Porcelain Letters.»—Slake 15 parts of fresh quicklime in 20
parts of water. Melt 50 parts of caoutchouc and 50 parts of linseed-oil
varnish together, and bring the mixture to a boil. While boiling,
pour the liquid on the slaked lime, little by little, under constant
stirring. Pass the mixture, while still hot, through muslin, to remove
any possible lumps, and let cool. It takes the cement 2 days to set
completely, but when dry it makes a joint that will resist a great
deal of strain. By thinning the mixture down with oil of turpentine, a
brilliant, powerfully adhesive varnish is obtained.

«Water-Glass Cements.»—I.—Water glass (sodium of potassium silicate),
which is frequently recommended for cementing glass, does not, as is
often asserted, form a vitreous connection between the joined surfaces;
and, in fact, some of the commercial varieties will not even dry, but
merely form a thick paste, which has a strong affinity for moisture.
Good 30° B. water glass is, however, suitable for mending articles that
are exposed to heat, and is best applied to surfaces that have been
gently warmed; when the pieces are put together they should be pressed
warmly, to expel any superfluous cement, and then heated strongly.

To repair cracked glasses or bottles through which water will leak,
water glasses may be used, the application being effected in the
following easy manner: The vessel is warmed to induce rarefaction of
the internal air, after which the mouth is closed, either by a cork
in the case of bottles, or by a piece of parchment or bladder if a
wide-mouthed vessel is under treatment.

While still hot, the outside of the crack is covered with a little
glass, and the vessel set aside to cool, whereupon the difference
between the pressure of the external and internal air will force the
cement into the fissure and close it completely. All that is then
necessary is to take off the cover and leave the vessel to warm for a
few hours. Subsequently rinse it out with lime water, followed by clean
water, and it will then hold any liquid, acids and alkaline fluids
alone excepted.

II.—When water glass is brought into contact with calcium chloride,
a calcium silicate is at once formed which is insoluble in water. It
seems possible that this reaction may be used in binding together
masses of sand, etc. The process indicated has long been used in the
preservation of stone which has become “weathered.” The stone is first
brushed with the water glass and afterwards with a solution of calcium
chloride. The conditions here are of course different.

Calcium chloride must not be confounded with the so-called “chloride of
lime” which is a mixture of calcium hypochlorite and other bodies.

«To Fasten Paper Tickets to Glass.»—To attach paper tickets to glass,
the employment of water glass is efficacious. Care should be taken
to spread this product on the glass and not on the paper, and then
to apply the paper dry, which should be done immediately. When the
solution is dry the paper cannot be {20} detached. The silicate should
be somewhat diluted. It is spread on the glass with a rag or a small
sponge.

«JEWELERS’ CEMENTS.»

Jewelers and goldsmiths require, for the cementing of genuine and
colored gems, as well as for the placing of colored folio under
certain stones, very adhesive gluing agents, which must, however,
be colorless. In this respect these are distinguished chiefly by the
so-called diamond cement and the regular jewelers’ cement. Diamond
cement is much esteemed by jewelers for cementing precious stones and
corals, but may also be employed with advantage for laying colored
fluxes of glass on white glass. The diamond cement is of such a nature
as to be able to remain for some time in contact with water without
becoming soft. It adheres best between glass or between precious
stones. It is composed as follows: Isinglass 8 parts, gum ammoniac 1
part, galbanum 1 part, spirit of wine 4 parts. Soak the isinglass in
water with admixture of a little spirit of wine and add the solution
of the gums in the remainder of the spirit of wine. Before use, heat
the diamond cement a little so as to soften it. Jewelers’ cement is
used for similar purposes as is the diamond cement, and is prepared
from: Isinglass (dry) 10 parts, mastic varnish 5 parts. Dissolve the
isinglass in very little water, adding some strong spirit of wine. The
mastic varnish is prepared by pouring a mixture of highly rectified
spirit of wine and benzine over finely powdered mastic and dissolving
it in the smallest possible quantity of liquid. The two solutions of
isinglass and mastic are intimately ground together in a porcelain dish.

«Armenian Cement.»—The celebrated “Armenian” cement, so called formerly
used by Turkish and Oriental jewelers generally, for setting precious
stones, “facing diamonds,” rubies, etc., is made as follows:

Mastic gum 10 parts
Isinglass (fish glue) 20 parts
Gum ammoniac 5 parts
Alcohol absolute 60 parts
Alcohol, 50 per cent 35 parts
Water 100 parts

Dissolve the mastic in the absolute alcohol; dissolve, by the aid of
gentle heat, on the water bath, the isinglass in the water, and add 10
parts of the dilute alcohol. Now dissolve the ammoniacum in the residue
of the dilute alcohol. Add the first solution to the second, mix
thoroughly by agitation and then add the solution of gum ammoniac and
stir well in. Finally put on the water bath, and keeping at a moderate
heat, evaporate the whole down to 175 parts.

«Cement for Enameled Dials.»—The following is a good cement for
enameled dials, plates, or other pieces: Grind into a fine powder
2 1⁠/⁠2 parts of dammar rosin and 2 1⁠/⁠2 parts of copal, using
colorless pieces if possible. Next add 2 parts of Venetian turpentine
and enough spirit of wine so that the whole forms a thick paste. To
this grind 3 parts of the finest zinc white. The mass now has the
consistency of prepared oil paint. To remove the yellow tinge of the
cement add a trifle of Berlin blue to the zinc white. Finally, the
whole is heated until the spirit of wine is driven off and a molten
mass remains, which is allowed to cool and is kept for use. Heat the
parts to be cemented.

«Watch-Lid Cement.»—The hardest cement for fixing on watch lids is
shellac. If the lids are exceedingly thin the engraving will always
press through. Before cementing it on the inside of the lid, in order
not to injure the polish, it is coated with chalk dissolved in alcohol,
which is first allowed to dry. Next melt the shellac on the stick, heat
the watch lid and put it on. After the engraving has been done, simply
force the lid off and remove the remaining shellac from the latter by
light tapping. If this does not remove it completely lay the lid in
alcohol, leaving it therein until all the shellac has dissolved. All
that remains to be done now is to wash out the watch lid.

«Jewelers’ Glue Cement.»—Dissolve on a water bath 50 parts of fish glue
in a little 95-per-cent alcohol, adding 4 parts, by weight, of gum
ammoniac. On the other hand, dissolve 2 parts, by weight, of mastic in
10 parts, by weight, of alcohol. Mix these two solutions and preserve
in a well-corked flask. For use it suffices to soften it on the water
bath.

«Casein Cements.»—

I.—Borax 5 parts
Water 95 parts
Casein, sufficient quantity.

Dissolve the borax in water and incorporate enough casein to produce a
mass of the proper consistency.

II.—The casein is made feebly alkaline by means of soda or potash lye
and {21} then subjected for about 24 hours to a temperature of 140° F.
Next follow the customary admixture, such as lime and water glass, and
finally, to accomplish a quicker resinification, substances containing
tannin are added. For tannic admixtures to the partially disintegrated
casein, slight quantities—about 1 per cent—of gallic acid, cutch, or
quercitannic acid are employed. The feebly alkaline casein cement
containing tannic acid is used in the well-known manner for the gluing
together of wood.

«For Metals.»—Make a paste with 16 ounces casein, 20 ounces slaked
lime, and 20 ounces of sand, in water.

«For Glass.»—I.—Dissolve casein in a concentrated solution of borax.

II.—Make a paste of casein and water glass.

«Pasteboard and Paper Cement.»—I.—Let pure glue swell in cold water;
pour and press off the excess; put on the water bath and melt. Paper
or other material cemented with this is then immediately, before the
cement dries, submitted to the action of formaldehyde and dried. The
cement resists the action of water, even hot.

II.—Melt together equal parts of good pitch and gutta percha. To 9
parts of this mass add 3 parts of boiled linseed oil and 1⁠/⁠5 part
litharge. The heat is kept up until, with constant stirring, an
intimate union of all the ingredients has taken place. The mixture is
diluted with a little benzine or oil of turpentine and applied while
still warm. The cement is waterproof.

III.—The _National Druggist_ says that experience with pasting or
cementing parchment paper seems to show that about the best agent
is casein cement, made by dissolving casein in a saturated aqueous
solution of borax.

IV.—The following is recommended for paper boxes:

Chloral hydrate 5 parts
Gelatin, white 8 parts
Gum arabic 2 parts
Boiling water 30 parts

Mix the chloral, gelatin, and gum arabic in a porcelain container, pour
the boiling water over the mixture and let stand for 1 day, giving it
a vigorous stirring several times during the day. In cold weather this
is apt to get hard and stiff, but this may be obviated by standing the
container in warm water for a few minutes. This paste adheres to any
surface whatever.

«Waterproof Cements for Glass, Stoneware, and Metal.»—I.—Make a paste
of sulphur, sal ammoniac, iron filings, and boiled oil.

II.—Mix together dry: Whiting, 6 pounds; plaster of Paris, 3 pounds;
sand, 3 pounds; litharge, 3 pounds; rosin, 1 pound. Make to a paste
with copal varnish.

III.—Make a paste of boiled oil, 6 pounds; copal, 6 pounds; litharge, 2
pounds; white lead, 1 pound.

IV.—Make a paste with boiled oil, 3 pounds; brickdust 2 pounds; dry
slaked lime, 1 pound.

V.—Dissolve 93 ounces of alum and 93 ounces of sugar of lead in water
to concentration. Dissolve separately 152 ounces of gum arabic in 25
gallons of water, and then stir in 62 1⁠/⁠2 pounds of flour. Then heat
to a uniform paste with the metallic salts, but take care not to boil
the mass.

VI.—For Iron and Marble to Stand in Heat.—In 3 pounds of water dissolve
first, 1 pound water glass and then 1 pound of borax. With the solution
make 2 pounds of clay and 1 pound of barytes, first mixed dry, to a
paste.

VII.—Glue to Resist Boiling Water.—Dissolve separately in water 55
pounds of glue and a mixture of 40 pounds of bichromate and 5 pounds of
alum. Mix as wanted.

VIII. (Chinese Glue).—Dissolve shellac in 10 times its weight of
ammonia.

IX.—Make a paste of 40 ounces of dry slaked lime 10 ounces of alum, and
50 ounces of white of egg.

X.—Alcohol 1,000 parts
Sandarac 60 parts
Mastic 60 parts
Turpentine oil 60 parts

Dissolve the gums in the alcohol and add the oil and stir in. Now
prepare a solution of equal parts of glue and isinglass, by soaking 125
parts of each in cold water until it becomes saturated, pouring and
pressing off the residue, and melting on the water bath. This should
produce a volume of glue nearly equal to that of the solution of gums.
The latter should, in the meantime, have been cautiously raised to
the boiling point on the water bath, and then mixed with the hot glue
solution.

It is said that articles united with this substance will stand the
strain of cold water for an unlimited time, and it takes hot water even
a long time to affect it. {22}

XI.—Burgundy pitch 6 parts
Gutta percha 1 part
Pumice stone, in fine powder 3 parts

Melt the gutta percha very carefully add the pumice stone, and lastly
the pitch, and stir until homogeneous.

Use while still hot. This cement will withstand water and dilute
mineral acids.

«LEATHER AND RUBBER CEMENTS.»

I.—Use a melted mixture of gutta percha and genuine asphalt, applied
hot. The hard-rubber goods must be kept pressed together until the
cement has cooled.

II.—A cement which is effective for cementing rubber to iron and which
is especially valuable for fastening rubber bands to bandsaw wheels is
made as follows: Powdered shellac, 1 part; strong water of ammonia,
10 parts. Put the shellac in the ammonia water and set it away in a
tightly closed jar for 3 or 4 weeks. By that time the mixture will
become a perfectly liquid transparent mass and is then ready for
use. When applied to rubber the ammonia softens it, but it quickly
evaporates, leaving the rubber in the same condition as before. The
shellac clings to the iron and thus forms a firm bond between the iron
and the rubber.

III.—Gutta percha white 1 drachm
Carbon disulphide 1 ounce

Dissolve, filter, and add:

India rubber 15 grains

Dissolve.

«Cement for Metal on Hard Rubber.»—I.—Soak good Cologne glue and boil
down so as to give it the consistency of joiners’ glue, and add with
constant stirring, enough sifted wood ashes until a homogeneous,
moderately thick mass results. Use warm and fit the pieces well
together while drying.

«How to Unite Rubber and Leather.»—II.—Roughen both surfaces, the
leather and the rubber, with a sharp glass edge; apply to both a
diluted solution of gutta percha in carbon bisulphide and let this
solution soak into the material. Then press upon each surface a skin
of gutta percha 1⁠/⁠10 of an inch in thickness between rolls. The two
surfaces are now united in a press, which should be warm but not hot.
This method should answer in all cases in which it is applicable. The
other prescription covers cases in which a press cannot be used. Cut
30 parts of rubber into small pieces, and dissolve it in 140 parts of
carbon bisulphide, the vessel being placed on a water bath of 30° C.
(86° F.). Further, melt 10 parts of rubber with 15 of colophony, and
add 35 parts of oil of turpentine. When the rubber has been completely
dissolved, the two liquids may be mixed. The resulting cement must be
kept well corked.

«To Fasten Rubber to Wood.»—I.—Make a cement by macerating virgin gum
rubber, or as pure rubber as can be had, cut in small pieces, in just
enough naphtha or gasoline to cover it. Let it stand in a very tightly
corked or sealed jar for 14 days, or a sufficient time to become
dissolved, shaking the mixture daily.

II.—Dissolve pulverized gum shellac, 1 ounce, in 9 1⁠/⁠2 ounces of
strong ammonia. This of course must be kept tightly corked. It will not
be as elastic as the first preparation.

III.—Fuse together shellac and gutta percha in equal weights.

IV.—India rubber 8 ounces
Gutta percha 4 ounces
Isinglass 2 ounces
Bisulphide of carbon 32 ounces

V.—India rubber 5 ounces
Gum mastic 1 ounce
Chloroform 3 ounces

VI.—Gutta percha 16 ounces
India rubber 4 ounces
Pitch 4 ounces
Shellac 1 ounce
Linseed oil 1 ounce

Amalgamate by heat.

VII.—Mix 1 ounce of oil of turpentine with 10 ounces of bisulphide of
carbon in which as much gutta percha as possible has been dissolved.

VIII.—Amalgamate by heat:

Gutta percha 100 ounces
Venice turpentine 80 ounces
Shellac 8 ounces
India rubber 2 ounces
Liquid storax 10 ounces

IX.—Amalgamate by heat:

India rubber 100 ounces
Rosin 15 ounces
Shellac 10 ounces

Then dissolve in bisulphide of carbon.

X.—Make the following solutions separately and mix:

(_a_) India rubber 5 ounces
Chloroform 140 ounces

(_b_) India rubber 5 ounces
Rosin 2 ounces
Venice turpentine 1 ounce
Oil of turpentine 20 ounces

{23}

«Cement for Patching Rubber Boots and Shoes.»—

I.—India rubber, finely chopped 100 parts
Rosin 15 parts
Shellac 10 parts
Carbon disulphide, q. s. to dissolve.

This will not only unite leather to leather, india rubber, etc., but
will unite rubber to almost any substance.

II.—Caoutchouc, finely cut 4 parts
India rubber, finely cut 1 part
Carbon disulphide 32 parts

Dissolve the caoutchouc in the carbon disulphide, add the rubber, let
macerate a few days, then mash with a palette knife to a smooth paste.
The vessel in which the solution is made in both instances above must
be kept tightly closed, and should have frequent agitations.

III.—Take 100 parts of crude rubber or caoutchouc, cut it up in small
bits, and dissolve it in sufficient carbon bisulphide, add to it 15
parts of rosin and 10 parts of gum lac. The user must not overlook the
great inflammability and exceedingly volatile nature of the carbon
bisulphide.

«Tire Cements.»—

I.—India rubber 15 grams
Chloroform 2 ounces
Mastic 1⁠/⁠2 ounce

Mix the india rubber and chloroform together, and when dissolved, the
mastic is added in powder. It is then allowed to stand a week or two
before using.

II.—The following is recommended as very good for cementing pneumatic
tires to bicycle wheels:

Shellac 1 ounce
Gutta percha 1 ounce
Sulphur 45 grains
Red lead 45 grains

Melt together the shellac and gutta percha, then add, with constant
stirring, the sulphur and red lead. Use while hot.

III.—Raw gutta percha 16 ounces
Carbon bisulphide 72 ounces
Eau de Cologne 2 2⁠/⁠3 ounces

This cement is the subject of an English patent and is recommended for
patching cycle and motor tires, insulating electric wires, etc.

IV.—A good thick shellac varnish with which a small amount of castor
oil has been mixed will be found a very excellent bicycle rim cement.
The formula recommended by Edel is as follows:

Shellac 1 pound
Alcohol 1 pint

Mix and dissolve, then add:

Castor oil 1⁠/⁠2 ounce

The castor oil prevents the cement from becoming hard and brittle.

A cement used to fasten bicycle tires may be made by melting together
at a gentle heat equal parts of gutta percha and asphalt. Apply hot.
Sometimes a small quantity each of sulphur and red lead is added (about
1 part of each to 20 parts of cement).

«Cements for Leather.»—

I.—Gutta percha 20 parts
Syrian asphalt, powdered 20 parts
Carbon disulphide 50 parts
Oil of turpentine 10 parts

The gutta percha, shredded fine, is dissolved in the carbon disulphide
and turpentine oil. To the solution add the asphalt and set away for
several days, or until the asphalt is dissolved. The cement should have
the consistency of honey. If the preparation is thinner than this let
it stand, open, for a few days. Articles to be patched should first be
washed with benzine.

II.—Glue 1 ounce
Starch paste 2 ounces
Turpentine 1 drachm
Water, a sufficient quantity.

Dissolve the glue in sufficient water with heat; mix the starch paste
with water; add the turpentine, and finally mix with the glue while hot.

III.—Soak for one day 1 pound of common glue in enough water to cover,
and 1 pound of isinglass in ale droppings. Then mix together and heat
gently until boiling. At this point add a little pure tannin and keep
boiling for an hour. If the glue and isinglass when mixed are too
thick, add water. This cement should be used warm and the jointed
leather pressed tightly together for 12 hours.

IV.—A waterproof cement for leather caoutchouc, or balata, is prepared
by dissolving gutta percha, caoutchouc, benzoin, gum lac, mastic,
etc., in some convenient solvent like carbon disulphide, chloroform,
ether, or alcohol. The best solvent, however, in the case of gutta
percha, is carbon disulphide and ether for mastic. The most favorable
proportions are as follows: Gutta percha, 200 to 300 parts to 100 parts
of the solvent, and 75 to 85 parts of mastic to 100 parts of ether.
From 5 to 8 parts of the former solution are mixed with 1 {24} part of
the latter, and the mixture is then boiled on the water bath, or in a
vessel fitted with a water jacket.

V.—Make a solution of 200 to 300 parts of caoutchouc, gutta percha,
india rubber, benzoin, or similar gum, in 1,000 parts of carbon
disulphide, chloroform, ether, or alcohol, and of this add 5 to 8 parts
to a solution of mastic (75 to 125 parts) in ether 100 parts, of equal
volume and boil together. Use hot water as the boiling agent, or boil
very cautiously on the water bath.

VI.—Forty parts of aluminum acetate, 10° B., 10 parts of glue, 10 parts
of rye flour. These materials are either to be simultaneously mixed and
boiled, or else the glue is to be dissolved in the aluminum acetate,
and the flour stirred into the solution. This is an excellent cement
for leather, and is used in so-called art work with leather, and with
leather articles which are made of several pieces. It is to be applied
warm.

«Rubber Cement for Cloth.»—The following formulas have been recommended:

I.—Caoutchouc, 5 parts; chloroform, 3 parts. Dissolve and add gum
mastic (powder) 1 part.

II.—Gutta percha, 16 parts; india rubber, 4 parts; pitch, 2 parts;
shellac, 1 part; linseed oil, 2 parts. Reduce the solids to small
pieces, melt together with the oil and mix well.

III.—The following cement for mending rubber shoes and tires will
answer similar purposes:

Caoutchouc in shavings 10 parts by weight
Rosin 4 parts by weight
Gum turpentine 40 parts by weight
Oil turpentine, enough.

Melt together first the caoutchouc and rosin, then add the gum
turpentine, and when all is liquefied, add enough of oil of turpentine
to preserve it liquid. A second solution is prepared by dissolving
together:

Caoutchouc 10 parts by weight
Chloroform 280 parts by weight

For use these two solutions are mixed. Wash the hole in the rubber shoe
over with the cement, then a piece of linen dipped in it is placed
over it; as soon as the linen adheres to the sole, the cement is then
applied as thickly as required.

«CEMENTS FOR METALS AND FOR ATTACHING VARIOUS SUBSTANCES TO METALS:»

«Cements for Iron.»—I.—To make a good cement for iron on iron, make a
thick paste, with water, of powdered iron, 60 parts; sal ammoniac, 2
parts, and sulphur flowers, 1 part. Use while fresh.

II.—Sulphur flowers, 6 parts; dry white lead 6 parts, and powdered
borax, 1 part. Mix by sifting and keep as a dry powder in a closed tin
box. To use, make into a thin paste with strong sulphuric acid and
press together immediately. This cement will harden in 5 days.

III.—Graphite 50 pounds
Whiting 15 pounds
Litharge 15 pounds

Make to a paste with a boiled oil.

IV.—Make a paste of white lead and asbestos.

V.—Make a paste of litharge and glycerine. Red lead may be added. This
also does for stone.

VI.—Make a paste of boiled oil of equal parts of white lead, pipe clay,
and black oxide of manganese.

VII.—Make iron filings to a paste with water glass.

VIII.—Sal ammoniac 4 ounces
Sulphur 2 ounces
Iron filings 32 ounces

Make as much as is to be used at once to a paste with a little water.
This remark applies to both the following dry recipes:

IX.—Iron filings 160 ounces
Lime 80 ounces
Red lead 16 ounces
Alum 8 ounces
Sal ammoniac 2 ounces

X.—Clay 10 ounces
Iron filings 4 ounces
Salt 1 ounce
Borax 1 ounce
Black oxide of manganese 2 ounces

XI.—Mix:

Iron filings 180 ounces
Lime 45 ounces
Salt 8 ounces

XII.—Mix:

Iron filings 140 ounces
Hydraulic lime 20 ounces
Sand 25 ounces
Sal ammoniac 3 ounces

Either of these last two mixtures is made into a paste with strong
vinegar just before use.

XIII.—Mix equal weights of zinc oxide and black oxide of manganese into
a paste with water glass.

XIV.—Copal varnish, 15 parts; hydrated lime, 10 parts; glue _de
nerfs_ (of sinews), 5 parts; fat drying oil, 5 parts; {25} powdered
turpentine, 3 parts; essence of turpentine, 2 parts. Dissolve the
glue _de nerfs_ on the water bath, add all the other substances, and
triturate intimately.

XV.—Copal varnish, 15 parts; powdered turpentine, 3 parts; essence
of turpentine, 2 parts; powdered fish glue, 3 parts; iron filings, 3
parts; ocher, 10 parts.

XVI.—To make a cement for cast iron, take 16 ounces cast-iron borings;
2 ounces sal ammoniac, and 1 ounce sulphur. Mix well and keep dry.
When ready to use take 1 part of this powder to 20 parts of cast-iron
borings and mix thoroughly into a stiff paste, adding a little water.

XVII.—Litharge 2 parts
Boiled linseed oil 2 parts
White lead 1 part
Copal 1 part

Heat together until of a uniform consistence and apply warm.

XVIII.—A cement for iron which is said to be perfectly waterproof and
fireproof is made by working up a mixture of equal weights of red lead
and litharge with glycerine till the mass is perfectly homogeneous and
has the consistency of a glazier’s putty. This cement is said to answer
well, even for very large iron vessels, and to be unsurpassable for
stopping up cracks in large iron pans of steam pipes.

«Cement for Metal, Glass, and Porcelain.»—A soft alloy is prepared by
mixing from 30 to 36 parts of copper precipitated in the form of a
fine brown powder, with sulphuric acid of a specific gravity of 1.85
in a cast-iron or porcelain mortar and incorporating by stirring with
75 parts of mercury, the acid being afterwards removed by washing with
water. In from 10 to 14 hours the amalgam becomes harder than tin, but
when heated to 692° F., it can be kneaded like wax. In this condition
it is applied to the surface to be cemented, and will fix them firmly
together on cooling.

Dissolve 1 drachm of gum mastic in 3 drachms of spirits of wine. In
a separate vessel containing water soak 3 drachms of isinglass. When
thoroughly soaked take it out of the water and put it into 5 drachms
of spirits of wine. Take a piece of gum ammoniacum the size of a large
pea and grind it up finely with a little spirits of wine and isinglass
until it has dissolved. Then mix the whole together with sufficient
heat. It will be found most convenient to place the vessel on a
hot-water bath. Keep this cement in a bottle closely stoppered, and
when it is to be used, place it in hot water until dissolved.

«Cements for Fastening Porcelain to Metal.»—I.—Mix equal parts of
alcohol (95 per cent) and water, and make a paste by incorporating
the liquid with 300 parts of finely pulverized chalk and 250 parts of
starch.

II.—Mix finely powdered burned lime, 300 parts, with powdered starch,
250 parts, and moisten the mixture with a compound of equal parts of
water and alcohol of 95 per cent until a paste results.

III.—Cement or plaster can be used if the surfaces are sufficiently
large; cement is the better article when the object may be exposed
to moisture or subjected to much pressure. A process which can be
recommended consists in mingling equal weights of chalk, brickdust,
clay, and Romain cement. These materials, pulverized and sifted are
incorporated with linseed oil in the proportion of half a kilo of oil
to 3 kilos of the mingled powder. The Romain or Romanic cement is so
designated from the district in France where the calcareous stone from
which it is prepared is found in considerable quantity. Although its
adhesive qualities are unquestioned, there are undoubtedly American
cements equally as good.

IV.—Acetate of lead, 46 1⁠/⁠2 parts by weight; alum, 46 1⁠/⁠2 parts by
weight; gum arabic, 76 parts by weight; flour, 500 parts by weight;
water, 2,000 parts by weight. Dissolve the acetate of lead and the alum
in a little water; on the other hand dissolve the gum arabic in water
by pouring, for instance, the 2 liters of boiling water on the gum
arabic reduced to powder. When the gum has dissolved, add the flour,
put all on the fire, and stir well with a piece of wood; then add the
solution of acetate of lead and the alum; agitate well so as to prevent
any lumps from forming; retire from the fire before allowing to boil.
This glue is used cold, does not peel off, and is excellent to make
wood, glass, cardboard, etc. adhere to metals.

«Cement for Leather and Iron.»—To face a cast-iron pulley with leather
apply acetic acid to the face of the pulley with a brush, which will
roughen it by rusting, and then when dry apply a cement made of 1 pound
of fish glue and 1⁠/⁠2 pound of common glue, melted in a mixture of
alcohol and water. The leather should then be placed on the pulley and
dried under pressure. {26}

«Amber Cements.»—I.—To solder together two pieces of yellow amber,
slightly heat the parts to be united and moisten them with a solution
of caustic soda; then bring the two pieces together quickly.

II.—Dissolve in a closed bottle 75 parts of cut-up caoutchouc in 60
parts of chloroform. Add 15 parts of mastic and let the mixture stand
in the cold until all has dissolved.

III.—Moisten the pieces to be joined with caustic potash and press
them together when warm. The union is so perfect that no trace of the
juncture is visible. A concentrated alcoholic solution of the rosin
over the amber, soluble in alcohol, is also employed for this purpose.
Another medium is a solution of hard and very finely powdered copal in
pure sulphuric ether. Coat both fractures, previously well cleaned,
with this solution and endeavor to combine them intimately by tying or
pressing.

IV.—In 30 parts by weight of copal dissolve 30 parts by weight of
alumina by means of a water bath. Bathe the surface to be cemented with
this gelatinous liquid, but very slightly. Unite the fractures and
press them together firmly until the mixture is dry.

«Acid-Proof Cements for Stoneware and Glass.»—I.—Mix with the aid of
heat equal weights of pitch, rosin, and plaster of Paris.

II.—Mix silicate of soda to a paste with ground glass.

III.—Mix boiled oil to a paste with china clay.

IV.—Mix coal tar to a paste with pipe clay.

V.—Mix boiled oil to a paste with quicklime.

VI.—Mix with the aid of heat: Sulphur, 100 pounds; tallow, 2 pounds;
rosin, 2 pounds. Thicken with ground glass.

VII.—Mix with the aid of heat: Rosin, 2 pounds; sulphur, 2 pounds;
brickdust, 4 pounds.

VIII.—Mix with the aid of heat 2 pounds of india rubber and 4 pounds of
oiled oil. Thicken with 12 pounds of pipe clay.

IX.—Fuse 100 pounds of india rubber with 7 pounds of tallow. Then make
to a paste with dry slaked lime and finally add 20 pounds of red lead.

X.—Mix with the aid of heat: Rosin, 24 pounds; red ocher, 8 pounds;
boiled oil, 2 pounds; plaster of Paris, 4 pounds.

«Acid-Proof Cement for Wood, Metals, etc.»—

I.—Powdered asbestos 2 parts
Ground baryta 1 part
Sodium water-glass solution 2 parts

Mix.

II.—To withstand hot nitric acid the following is used:

Sodium water-glass solution 2 parts
Sand 1 part
Asbestos 1 part

Mix.

III.—Asbestos 2 parts
Sulphate of barium 3 parts
Silicate of sodium 2 parts

By mixing these ingredients a cement strong enough to resist the
strongest nitric acid will be obtained.

IV.—If hot acids are dealt with, the following mixture will be found to
possess still more resistant powers:

Silicate of sodium (50° Baumé) 2 parts
Fine sand 1 part
Asbestos 1 part

Both these cements take a few hours to set. If the cement is wanted to
set at once, use silicate of potassium, instead of silicate of sodium.
This mixture will be instantly effective and possesses the same power
of resistance as the other.

«Directions for Repairing Broken Glass, Porcelain, Bric-à-Brac.»—Broken
glass, china, bric-à-brac, and picture frames, not to name casts,
require each a different cement—in fact, several different cements.
Glass may be beautifully mended to look at, but seldom so as to be
safely used. For clear glass the best cement is isinglass dissolved in
gin. Put 2 ounces of isinglass in a clean, wide-mouthed bottle, add
half a pint of gin, and set in the sun until dissolved. Shake well
every day, and before using strain through double lawn, squeezing very
gently.

Spread a white cloth over the mending table and supply it with plenty
of clean linen rags, strong rubber bands, and narrow white tape,
also a basin of tepid water and a clean soft towel. Wash the broken
glass very clean, especially along the break, but take care not to
chip it further. Wet both broken edges well with the glue, using a
camel’s-hair pencil. Fit the break to a nicety, then slip on rubber
bands length- and cross-wise, every way they will hold. If they will
not hold true as upon a stemmed {27} thing, a vase or jug or scent
bottle, string half a dozen bands of the same size and strength upon a
bit of tape, and tie the tape about neck or base before beginning the
gluing. After the parts are joined slip another tape through the same
bands and tie it above the fracture; thus with all their strength the
bands pull the break together. The bands can be used thus on casts of
china—in fact, to hold anything mendable. In glass mending the greater
the pressure the better—if only it stops short of the breaking point.
Properly made the isinglass cement is as clear as water. When the
pieces fit true one on the other the break should be hardly visible, if
the pressure has been great enough to force out the tiny bubbles, which
otherwise refract the light and make the line of cleavage distressingly
apparent. Mended glass may be used to hold dry things—as rose leaves,
sachets, violet powder, even candies and fruits. But it will not bear
to have any sort of liquid left standing in it, nor to be washed beyond
a quick rinsing in tepid water. In wiping always use a very soft towel,
and pat the vessel dry with due regard to its infirmities.

Mend a lamp loose in the collar with sifted plaster of Paris mixed to a
very soft paste with beaten white of egg. Have everything ready before
wetting up the plaster, and work quickly so it may set in place. With
several lamps to mend wet enough plaster for one at a time. It takes
less than 5 minutes to set, and is utterly worthless if one tries
working it over. Metal work apart from the glass needs the soldering
iron. Dust the break well with powdered rosin, tie the parts firmly
together, lay the stick of solder above the break, and fetch the iron
down on it lightly but firmly. When the solder cools, remove the melted
rosin with a cloth dipped in alcohol.

Since breakables have so unhappy a knack of fracturing themselves in
such fashion they cannot possibly stand upright, one needs a sand box.
It is only a box of handy size with 8 inches of clean, coarse sand in
the bottom. Along with it there should be some small leaden weights,
with rings cast in them, running from an ounce to a quarter pound. Two
of each weight are needed. In use, tapes are tied to the rings, and
the pair of weights swung outside the edges of the box, so as to press
in place the upper part of a broken thing to which the tapes have been
fastened.

Set broken platters on edge in the sand box with the break up. The
sand will hold them firm, and the broken bit can be slapped on. It
is the same with plates and saucers. None of these commonly requires
weighting. But very fine pieces where an invisible seam is wanted
should be held firm until partly set, then have the pair of heaviest
weights accurately balanced across the broken piece. The weights are
also very useful to prop and stay topheavy articles and balance them so
they shall not get out of kilter. A cup broken, as is so common with
cups, can have the tape passed around it, crossing inside the handle,
then be set firmly in the sand, face down, and be held by the hanging
weights pulling one against the other.

The most dependable cement for china is pure white lead, ground
in linseed oil, so thick it will barely spread smoothly with a
knife. Given time enough to harden (some 3 months), it makes a seam
practically indestructible. The objection to it is that it always shows
in a staring white line. A better cement for fine china is white of egg
and plaster. Sift the plaster three times and tie a generous pinch of
it loosely in mosquito netting. Then beat the egg until it will stick
to the plaster. Have the broken edge very clean, cover both with the
beaten egg, dust well with the plaster, fit together at once, tie,
using rubber bands if possible, wrap loosely in very soft tissue paper,
and bury head and ears in the sand box, taking care that the break lies
so that the sand will hold it together. Leave in the box 24 hours.
After a week the superfluous plaster may be gently scraped away.

«General Formulas for Cements for Repairing Porcelain, Glassware,
Crockery, Plaster, and Meerschaum.»—I.—An excellent cement for joining
broken crockery and similar small articles can be made by melting 4 or
5 parts of rosin (or, better still, gum mastic) with 1 part of beeswax
in an iron spoon or similar vessel. Apply while hot. It will not stand
great heat.

II.—An excellent cement for porcelain and stoneware is obtained by
mixing 20 parts of fish glue with an equal weight of crystallizable
acetic acid and evaporate the mixture carefully to a syrupy consistency
so that it forms a gelatinous mass on cooling. For use the cement thus
obtained is made liquid again by heating and applied to the fracture
with a brush. The pieces should now be pressed firmly together, by
winding a twine tightly around them, until the cement has hardened.

III.—For luting vessels made of glass, {28} porcelain, etc., which
are to be used to hold strong acids, a mixture of asbestos powder,
water glass, and an indifferent powder (permanent white, sand, etc.)
is recommended. To begin with, asbestos powder is made into a pulp
with three or four times the quantity (weight) of a solution of soda
water glass (of 30° B.). The same is exceedingly fat and plastic, but
is not very well suited for working, as it shrinks too much and cracks
when drying. By an addition of fine writing sand of the same weight
as the asbestos used, the mass can be made less fat, so as to obviate
shrinking, without detracting from the plasticity. Small vessels were
molded from it and dried in the air, to be tested afterwards. Put in
water, the hardened mass becomes soft again and falls apart. Brought
into contact, however, with very strong mineral acids, it becomes even
firmer and withstands the liquid perfectly. Concentrated nitric acid
was kept in such small vessels without the mass being visibly attacked
or anything penetrating it. The action of the acid manifestly has the
effect that silicic acid is set free from the water glass in excess,
which clogs up the pores entirely and contributes to the lutation.
Later on, the mass cannot be dissolved by pure water any more. The mass
is also highly fireproof. One of the molded bodies can be kept glowing
in a Bunsen gas flame for about half a day after treatment with acid,
without slagging in the least. For many purposes it ought to be welcome
to have such a mass at hand. It cannot be kept ready for use, however,
as it hardens a few hours after being prepared; if potash water glass
is used, instead of the soda composition, this induration takes place
still more quickly.

IV.—Cement for Glass, Porcelain, etc.—

Isinglass (fish glue) 50 parts
Gum ammoniac 4 parts
Gum mastic 2 parts
Alcohol, 95 per cent 10 parts
Water, q. s.

Soak the isinglass in cold water over night, or until it has become
swollen and soft throughout. In the morning throw off any superfluous
fluid and throw the isinglass on a clean towel or other coarse cloth,
and hang it up in such a way that any free residual water will drain
away. Upon doing this thoroughly depends, in a great measure, the
strength of the cement. When the gelatin has become thoroughly drained
put it into a flask or other container, place it in the water bath and
heat carefully until it becomes fluid, being careful not to let it come
to a boil, as this injures its adhesive properties (the same may be
said in regard to glues and gelatins of all kinds). Dissolve the gums
in the alcohol and add the solution to the gelatin after removing the
same from the water bath, and letting it cool down to about 160° F.
Stir well together or mix by agitation.

The following precautions must be observed: 1. Both surfaces to be
joined must be absolutely clean, free from dust, dirt, grease, etc.
2. Where the cement is one that requires the application of heat
before use, the objects to be united should also _be heated to a point
at least as high as the melting point of the cement_. Otherwise, the
cement on application is chilled and consequently fails to make a
lasting joint. 3. The thinner the layer of cement the stronger the
joint; avoid, therefore, using too much of the binding material. Cover
both surfaces to be united, coapt them exactly, and press together as
closely as possible. In this manner the thinnest possible layer is
secured. 4. Bind the parts securely together, and let remain without
loosening or attempting to use the article for 2 or 3 days or longer. A
liquid cement acquires its full strength only after evaporation of the
fluids used as solvents, and this can occur only from the infinitesimal
line of exposed surface.

V.—Liquid Porcelain Cement.—Fish glue, 20 parts; glass acetic acid, 20
parts; heat together until the mass gelatinizes on cooling.

VI.—Take 1 ounce of Russian isinglass, cut in small pieces, and bruise
well; then add 6 ounces of warm water, and leave it in a warm place
for from 24 to 48 hours. Evaporate the resulting solution to about 3
ounces. Next dissolve 1⁠/⁠2 ounce of mastic in 4 ounces of alcohol,
and add the mastic solution to the isinglass in small quantities at a
time, continuing the heat and stirring well. While still hot strain the
liquid through muslin.

VII.—For optical glasses, Canada balsam is employed, the two pieces
being firmly pressed together. After a while, especially by humidity,
punctures will form, and the glass is separated by a mist of varying
reflexes, while in certain climates the heat will melt the balsam. For
all other glass articles which require only simple treatment, such as
knobs of covers, plates, etc., silicate of potash is excellent.

VIII.—Glass Cement.—Dissolve in 150 parts of acetic acid of 96 per
cent, 100 {29} parts of gelatin by the use of heat, and add ammonium
bichromate, 5 parts. This glue must be kept away from the light.

IX.—White glue 10 parts
Potassium bichromate 2 parts
Water 100 parts

The glue is dissolved in a portion of the water by the aid of heat,
the bichromate in the remainder, and the liquids mixed, the mixing
being done in a feebly lighted place, and the mixture is then kept
in the dark. It is applied in feeble light, being reliquefied by
gentle heat, and the glass, the fractured pieces being tightly clamped
together, is then exposed to a strong light for some time. By this
exposure the cement becomes insoluble. This is waterproof cement for
glass.

X.—Diamond Glass Cement.—Dissolve 100 parts of fish glue in 150 parts
of 90 per cent alcohol and add, with constant stirring, 200 parts of
powdered rosin. This cement must be preserved in absolutely tight
bottles, as it solidifies very quickly.

XI.—To unite objects of crystal dissolve 8 parts of caoutchouc and 100
parts of gum mastic in 600 parts of chloroform. Set aside, hermetically
closed, for 8 days; then apply with a brush, cold.

XII.—To make a transparent cement for glass, digest together for a week
in the cold 1 ounce of india rubber, 67 ounces of chloroform, and 40
ounces of mastic.

XIII.—A mixture of traumaticin, a solution of caoutchouc in chloroform,
and a concentrated solution of water glass make a capital cement for
uniting articles of glass. Not only is the joint very strong, but it
is transparent. Neither changes of temperature nor moisture affect the
cement.

XIV.—A transparent cement for porcelain is prepared by dissolving 75
parts of india rubber, cut into small pieces, in a bottle containing
60 parts chloroform; to this add 15 parts green mastic. Let the
bottle stand in the cold until the ingredients have become thoroughly
dissolved.

XV.—Some preparations resist the action of heat and moisture a short
time, but generally yield very quickly. The following cement for glass
has proven most resistant to liquids and heat:

Silver litharge 1,000 parts
White lead 50 parts
Boiled linseed oil 3 parts
Copal varnish 1 part

Mix the lead and litharge thoroughly, and the oil and copal in the
same manner, and preserve separately. When needed for use, mix in
the proportions indicated (150 parts of the powder to 4 parts of the
liquid) and knead well together. Apply to the edges of the glass, bind
the broken parts together, and let stand for from 24 to 48 hours.

XVI.—To reunite plaster articles dissolve small pieces of celluloid in
ether; in a quarter of an hour decant, and use the pasty deposit which
remains for smearing the edges of the articles. It dries rapidly and is
insoluble in water.

XVII.—To Mend Wedgwood Mortars.—It is easy enough to mend mortars so
that they may be used for making emulsions and other light work which
does not tax their strength too much. But a mended mortar will hardly
be able to stand the force required for powdering hard substances. A
good cement for mending mortars is the following:

_a._—Glass flour elutriated 10 parts
Fluorspar, powdered and elutriated 20 parts
Silicate of soda 60 parts

Both glass and fluorspar must be in the finest possible condition,
which is best done by shaking each in fine powder, with water allowing
the coarser particles to deposit, and then to pour off the remainder,
which holds the finest particles in suspension. The mixture must be
made very rapidly by quick stirring, and when thoroughly mixed must be
at once applied. This is said to yield an excellent cement.

_b._—Freshly burnt plaster of Paris 5 parts
Freshly burnt lime 1 part
White of egg, sufficient.

Reduce the first two ingredients to a very fine powder and mix them
well; moisten the two surfaces to be united with a small quantity of
white of egg to make them adhesive; then mix the powder very rapidly
with the white of egg and apply the mixture to the broken surfaces. If
they are large, two persons should do this, each applying the cement
to one portion. The pieces are then firmly pressed together and left
undisturbed for several days. The less cement is used the better will
the articles hold together.

_c._—If there is no objection to dark-colored cement, the very best
that can be used is probably marine glue. This is made thus: Ten parts
of caoutchouc or india rubber are dissolved in 120 parts of benzine
or petroleum naphtha, with {30} the aid of a gentle heat. When the
solution is complete, which sometimes requires from 10 to 14 days,
20 parts of asphalt are melted in an iron vessel and the caoutchouc
solution is poured in very slowly in a fine stream and under continued
heating, until the mass has become homogeneous and nearly all the
solvent has been driven off. It is then poured out and cast into
greased tin molds. It forms dark brown or black cakes, which are very
hard to break. This cement requires considerable heat to melt it; and
to prevent it from being burnt it is best to heat a capsule containing
a piece of it first on a water bath until the cake softens and begins
to be liquid. It is then carefully wiped dry and heated over a naked
flame, under constant stirring, up to about 300° F. The edges of the
article to be mended should, if possible, also be heated to at least
212° F., so as to permit the cement to be applied at leisure and with
care. The thinner the cement is applied the better it binds.

«Meerschaum Cements.»—I.—If the material is genuine (natural)
meerschaum a lasting joint can be made between the parts by proceeding
as follows: Clean a clove or two of garlic (the fresher the better) by
removing all the outside hull of skin; throw into a little mortar and
mash to a paste. Rub this paste over each surface to be united and join
quickly. Bring the parts as closely together as possible and fasten in
this position. Have ready some boiling fresh milk; place the article in
it and continue the boiling for 30 minutes. Remove and let cool slowly.
If properly done, this makes a joint that will stand any ordinary
treatment, and is nearly invisible. For composition, use a cement made
of quicklime, rubbed to a thick cream with egg albumen.

II.—Mix very fine meerschaum shavings with albumen or dissolve casein
in water glass, stir finely powdered magnesia into the mass, and use
the cement at once. This hardens quickly.

«Asbestos Cement.»—Ground asbestos may be made into a cement which
will stand a high degree of heat by simply mixing it with a solution
of sodium silicate. By subsequent treatment with a solution of calcium
chloride the mass may be made insoluble, silicate of calcium being
formed.

A cement said to stand a high degree of heat and to be suitable for
cementing glass, porcelain, or other vessels intended to hold corrosive
acids, is this one:

I.—Asbestos 2 parts
Barium sulphate 3 parts
Sodium silicate 2 parts

By mixing these ingredients a cement strong enough to resist the
strongest nitric acid will be obtained. If hot acids are dealt with,
the following mixture will be found to possess still more resistant
powers:

II.—Sodium silicate 2 parts
Fine sand 1 part
Asbestos powder 1 part

Both these cements take a few hours to set. If the cement is wanted to
set at once, use potassium silicate instead of sodium silicate. This
mixture will be instantly effective, and possesses the same power of
resistance as the other.

«Parisian Cement.»—Mix 1 part of finely ground glass powder, obtained
by levigation, with 3 parts of finely powdered zinc oxide rendered
perfectly free from carbonic acid by calcination. Besides prepare a
solution of 1 part, by weight, of borax in a very small quantity of
hot water and mix this with 50 parts of a highly concentrated zinc
chloride solution of 1.5 to 1.6 specific gravity. As is well known the
mixture of this powder with the liquid into a soft uniform paste is
accomplished only immediately before use. The induration to a stonelike
mass takes place within a few minutes, the admixture of borax retarding
the solidification somewhat. The pure white color of the powder may be
tinted with ocher, manganese, etc., according to the shade desired.

«Strong Cement.»—Pour over well-washed and cleaned casein 12 1⁠/⁠2
parts of boiled linseed oil and the same amount of castor oil. Boil.
Stir actively and add a small amount of a saturated aqueous solution of
alum; remove from the fire and set aside. After a while a milky looking
fluid will separate and rise. This should be poured off. To the residue
add 120 parts of rock candy syrup and 6 parts of dextrin.

«A Cheap and Excellent Cement.»—A cheap and excellent cement, insoluble
after drying in water, petroleum, oils, carbon disulphide, etc., very
hard when dry and of very considerable tensile strength, is composed
of casein and some tannic-acid compound, as, for instance, calcium
tannate, and is prepared as follows:

First, a tannin solution is prepared either by dissolving a tannin
salt, or by extraction from vegetable sources (as barks from certain
trees, etc.), to which {31} is added clear lime water (obtained by
filtering milk of lime, or by letting the milk stand until the lime
subsides) until no further precipitation occurs, and red litmus paper
plunged in the fluid is turned blue. The liquid is now separated
from its precipitate, either by decantation or otherwise, and the
precipitate is dried. In operating with large quantities of the
substance, this is done by passing a stream of atmospheric air through
the same. The lime tannate obtained thus is then mixed with casein in
proportions running from 1:1 up to 1:10, and the mixture, thoroughly
dried, is milled into the consistency of the finest powder. This
powder has now only to be mixed with water to be ready for use, the
consistency of the preparation depending upon the use to which it is to
be put.

«Universal Cement.»—Take gum arabic, 100 parts, by weight; starch, 75
parts, by weight; white sugar, 21 parts, by weight; camphor, 4 parts,
by weight. Dissolve the gum arabic in a little water; also dissolve the
starch in a little water. Mix and add the sugar and camphor. Boil on
the water bath until a paste is formed which, on coating, will thicken.

«Cement for Ivory.»—Melt together equal parts of gutta percha and
ordinary pitch. The pieces to be united have to be warmed.

«Cement for Belts.»—Mix 50 parts, by weight, of fish glue with equal
parts of whey and acetic acid. Then add 50 parts, by weight, of garlic
in paste form and boil the whole on the water bath. At the same time
make a solution of 100 parts, by weight, of gelatin in the same
quantity of whey, and mix both liquids. To the whole add, finally,
50 parts, by weight, of 90-per-cent alcohol and, after filtration,
a cement is obtained which can be readily applied with a brush and
possesses extraordinary binding qualities.

«Cement for Chemical Apparatus.»—Melt together 20 parts of gutta
percha, 10 parts of yellow wax, and 30 parts of shellac.

«Size Over Portland Cement.»—The best size to use on Portland cement
molding for wall paper would ordinarily be glue and alum size put on
thin and warm, made in proportion of 1⁠/⁠2 pound of glue and same
weight of alum dissolved in separate pails, then poured together.

«Aquarium Cements.»—

I.—Litharge 3 ounces
Fine white sand 3 ounces
Plaster of Paris 3 ounces
Rosin, in fine powder 1 ounce
Linseed oil, enough.
Drier, enough.

Mix the first three ingredients, add sufficient linseed oil to make a
homogeneous paste, and then add a small quantity of drier. This should
stand a few hours before it is used. It is said that glass joined to
iron with this cement will break before it will come loose.

II.—Litharge 1 ounce
Fine white sand 1 ounce
Plaster of Paris 1 ounce
Manganese borate 20 grains
Rosin, in fine powder 3 1⁠/⁠2 pounds
Linseed varnish oil, enough.

III.—Take equal parts of flowers of sulphur, ammonium chloride, and
iron filings, and mix thoroughly with boiled linseed oil. Finally, add
enough white lead to form a thin paste.

IV.—Powdered graphite 6 parts
Slaked lime 3 parts
Barium sulphate 8 parts
Linseed varnish oil 7 parts

V.—Simply mix equal parts of white and red lead with a little
kettle-boiled linseed oil.

«Substitute for Cement on Grinder Disks.»—A good substitute in place of
glue or various kinds of cement for fastening emery cloth to the disks
of grinders of the Gardner type is to heat or warm the disk and apply a
thin coating of beeswax; then put the emery cloth in place and allow to
set and cool under pressure.

«Knockenplombe.»—If 1 part of thymol be mixed with 2 parts of iodoform
we obtain a substance that retains its fluidity down to 72° C.
(161.6° F.). If the temperature be carried down to 60° C. (140° F.)
it suddenly becomes solid and hard. If, in its liquid condition, this
substance be mixed intimately with an equal quantity of calcined bone,
it forms a cement that can be molded or kneaded into any shape, that,
at the temperature of the body (98° F.), becomes as hard as stone, a
fact that suggests many useful purposes to which the mixture may be put.

«Cement for General Use.»—Take gum arabic, 100 parts, by weight;
starch, 75 {32} parts by weight; white sugar, 21 parts, by weight;
camphor, 4 parts, by weight. Dissolve the gum arabic in a little water.
On the other hand, dissolve the starch also in some water. When this is
done add the sugar and the camphor and put in a water bath. Boil until
a paste is formed, which must be rather thin, because it will thicken
on cooling.

«Strong Cement.»—Pour over well-washed and cleaned casein 12 1⁠/⁠2
parts of boiled linseed oil and the same amount of castor oil, put on
the fire and bring to a boil; stir actively and add a small amount of
a saturated aqueous solution of alum; remove from the fire and set
aside. After standing a while a milky-looking fluid will separate at
the bottom and rise to the top. This should be poured off and to the
residue add 120 parts of rock-candy syrup and 6 parts of dextrine.

«Syndeticon.»—I.—Slake 100 parts of burnt lime with 50 parts of water,
pour off the supernatant water; next, dissolve 60 parts of lump sugar
in 160 parts of water, add to the solution 15 parts of the slaked
lime, heat to 70° or 80° C. (158° to 176° F.), and set aside, shaking
frequently. Finally dissolve 50 to 60 parts of genuine Cologne glue in
250 parts of the clear solution.

II.—A solution of 10 parts gum arabic and 30 parts of sugar in 100
parts of soda water glass.

III.—A hot solution of 50 parts of Cologne glue in 60 parts of a
20-per-cent aqueous calcium-chloride solution.

IV.—A solution of 50 parts of Cologne glue in 60 parts of acetic acid.

V.—Soak isinglass (fish bladder) in acetic acid of 70 per cent until it
swells up, then rub it up, adding a little water during the process.

«“Shio Liao.”»—Under this name the Chinese manufacture an excellent
cement which takes the place of glue, and with which gypsum, marble,
porcelain, stone, and stoneware can be cemented. It consists of the
following parts (by weight): Slaked powdered lime, 54 parts; powdered
alum, 6 parts; and fresh, well-strained blood, 40 parts. These
materials are stirred thoroughly until an intimately bound mass of
the consistency of a more or less stiff salve is obtained. In paste
form this mass is used as cement; in a liquid state it is employed for
painting all sorts of articles which are to be rendered waterproof and
durable. Cardboard covers, which are coated with it two or three times,
become as hard as wood. The Chinese paint their houses with “shio liao”
and glaze their barrels with it, in which they transport oil and other
greasy substances.

«LUTES.»

Lutes always consist of a menstruum and dissolved or suspended solids,
and they must not be attacked by the gases and liquids coming in
contact with them. In some cases the constituents of the lute react to
form a more strongly adhering mass.

The conditions of application are, in brief:

(_a_) Heating the composition to make it plastic until firmly fixed in
place.

(_b_) Heating the surfaces.

(_c_) Applying the lute with water or a volatile solvent, which is
allowed to volatilize.

(_d_) Moistening the surfaces with water, oil, etc. (the menstruum of
the lute itself).

(_e_) Applying the lute in workable condition and the setting taking
place by chemical reactions.

(_f_) Setting by hydration.

(_g_) Setting by oxidation.

These principles will be found to cover nearly all cases.

Joints should not be ill-fitting, depending upon the lute to do what
the pipes or other parts of the apparatus should do. In most cases one
part of the fitting should overlap the other, so as to make a small
amount of the lute effective and to keep the parts of the apparatus
rigid, as a luted joint is not supposed to be a particularly strong
one, but rather one quickly applied, effective while in place and
easily removed.

Very moderate amounts of the lute should be used, as large amounts are
likely to develop cracks, be rubbed off, etc.

A classification may be given as follows:

(1) Plaster of Paris.

(2) Hydraulic cement.

(3) Clay.

(4) Lime.

(5) Asphalt and pitch.

(6) Rosin.

(7) Rubber.

(8) Linseed oil.

(9) Casein and albumen.

(10) Silicates of soda and oxychloride cements.

(11) Flour and starch.

(12) Miscellaneous, including core compounds.

I. Plaster of Paris is, of course, often used alone as a paste; which
quickly {33} solidifies, for gas and wood distillation retorts, etc.,
and similar places where quickness of setting is requisite. It is more
often, however, used with some fibrous material to give it greater
strength. Asbestos is the most commonly used material of these, as it
will stand a high temperature. When that is not so important, straw,
plush trimmings, hair, etc., are used as binders, while broken stone,
glass, and various mineral substances are used as fillers, but they do
not add anything to the strength. These lutes seem to be particularly
suitable for oil vapors and hydrocarbon gases.

Formulas:

(1) Plaster and water.
(2) Plaster (wet) and asbestos.
(3) Plaster (wet) and straw.
(4) Plaster (wet) and plush trimmings.
(5) Plaster (wet) and hair.
(6) Plaster (wet) and broken stone, etc.

II. Hydraulic Cement.—Cement is used either alone or with sand,
asbestos, etc. These lutes are suitable for nitric acid. When used
with substances such as rosin or sulphur, cement is probably employed
because it is in such a fine state of division and used as a filler and
not because of any powers of setting by hydration.

Formulas:

(1) Cement—neat.
(2) Cement and asbestos.
(3) Cement and sand.

III. Clay.—This most frequently enters into the composition of lutes as
a filler, but even then the very finely divided condition of certain
grades renders it valuable, as it gives body to a liquid, such as
linseed oil, which, unless stiffened, would be pervious to a gas,
the clay in all cases being neutral. Thus, for luting pipes carrying
chlorine, a stiff paste of clay and molasses has been suggested by
Theo. Köller in _Die Surrogate_, but it soon gives way.

Formulas:

(1) Clay and linseed oil.
(2) Same, using fire clay.
(3) Clay and molasses.

(1) Is suitable for steam, etc.; (2) for chlorine, and (3) for oil
vapors.

IV. Lime is used in the old lute known as putty, which consists of
caustic lime and linseed oil. Frequently the lime is replaced by chalk
and china clay, but the lime should be, in part at least, caustic, so
as to form a certain amount of lime soap. Lime is also used in silicate
and casein compositions, which are very strong and useful, but will be
described elsewhere.

Formulas:

(1) Lime and boiled oil to stiff mass.
(2) Clay, etc., boiled oil to stiff mass.

V. Asphalt and Pitch.—These substances are used in lutes somewhat
interchangeably. As a rule, pitch makes the stronger lutes. Tar is
sometimes used, but, because of the light oils and, frequently, water
contained, it is not so good as either of the others.

Asphalt dissolved in benzol is very useful for uniting glass for
photographic, microscopical, and other uses. Also for coating wood,
concrete, etc., where the melted asphalt would be too thick to cover
well. Benzol is the cheapest solvent that is satisfactory for this
purpose, as the only one that is cheaper would be a petroleum naphtha,
which does not dissolve all the constituents of the asphalt. For
waterproofing wood, brick, concrete, etc., melted asphalt alone is
much used, but when a little paraffine is added, it improves its
waterproofing qualities, and in particular cases boiled oil is also
added to advantage.

Formulas:

1. Refined lake asphalt.

2. Asphalt 4 parts
Paraffine 1 part

3. Asphalt 10 parts
Paraffine 2 parts
Boiled oil 1 part

Any of these may be thinned with hot benzol or toluol. Toluol is
less volatile than benzol and about as cheap, if not cheaper, the
straw-colored grades being about 24 cents per gallon.

Examples of so-called “stone cement” are:

4. Pitch 8 parts
Rosin 6 parts
Wax 1 part
Plaster 1⁠/⁠4 to 1⁠/⁠2 part

5. Pitch 8 parts
Rosin 7 parts
Sulphur 2 parts
Stone powder 1 part

These compositions are used to unite slate slabs and stoneware for
domestic, engineering, and chemical purposes. Various rosin and pitch
mixtures are used for these purposes, and the proportions of these two
ingredients are determined by the consistency desired. Sulphur and
stone powder are added to prevent the formation of cracks, sulphur
acting chemically and stone powder mechanically. {34} Where the lute
would come in contact with acid or vapors of the same, limestone should
not be the powder used, otherwise it is about the best. Wax is a useful
ingredient to keep the composition from getting brittle with age.

A class of lutes under this general grouping that are much used are
so-called “marine glues” (q. v.). They must be tough and elastic. When
used for calking on a vessel they must expand and contract with the
temperature and not crack or come loose.

Formulas:

6. Pitch 3 parts
Shellac 2 parts
Pure crude rubber 1 part

7. Pitch 1 part
Shellac 1 part
Rubber substitute 1 part

These are used by melting over a burner.

VI. Rosin, Shellac, and Wax.—A strong cement, used as a stone cement,
is:

1. Rosin 8 parts
Wax 1 part
Turpentine 1 part

It has little or no body, and is used in thin layers.

For nitric and hydrochloric acid vapors:

2. Rosin 1 part
Sulphur 1 part
Fire clay 2 parts

Sulphur gives great hardness and permanency to rosin lutes, but this
composition is somewhat brittle.

Good waterproof lutes of this class are:

3. Rosin 1 part
Wax 1 part
Powdered stone 2 parts

4. Shellac 5 parts
Wax 1 part
Turpentine 1 part
Chalk, etc. 8 to 10 parts

For a soft air-tight paste for ground-glass surfaces:

5. Wax 1 part
Vaseline 1 part

6. A strong cement, without body, for metals (other than copper or
alloys of same), porcelain, and glass is made by letting 1 part of
finely powdered shellac stand with 10 parts of ammonia water until
solution is effected.

VII. Rubber.—Because of its toughness, elasticity, and resistance to
alterative influences, rubber is a very useful constituent in lutes,
but its price makes its use very limited.

Leather Cement.

1. Asphalt 1 part
Rosin 1 part
Gutta percha 4 parts
Carbon disulphide 20 parts

To stand acid vapors:

2. Rubber 1 part
Linseed oil 3 parts
Fire clay 3 parts

3. Plain Rubber Cement.—Cut the crude rubber in small pieces and then
add the solvent. Carbon disulphide is the best, benzol good and much
cheaper, but gasoline is probably most extensively used because of its
cheapness.

4. To make corks and wood impervious to steam and water, soak them in
a rubber solution as above; if it is desired to protect them from oil
vapors, use glue composition. (See Section IX.)

VIII. Linseed Oil.—This is one of the most generally useful substances
we have for luting purposes, if absorbed by a porous substance that is
inert.

Formulas: 1. China clay of general utility for aqueous vapors.

Linseed oil of general utility for aqueous vapors.

2. Lime forming the well-known putty.

Linseed oil forming the well-known putty.

3. Red or white lead and linseed oil.

These mixtures become very strong when set and are best diluted with
powdered glass, clay, or graphite. There are almost an endless number
of lutes using metallic oxides and linseed oil. A very good one, not
getting as hard as those containing lead, is:

4. Oxide of iron and linseed oil.

IX. Casein, Albumen, and Glue.—These, if properly made, become very
tough and tenacious; they stand moderate heat and oil vapors, but not
acid vapors.

1. Finely powdered casein 12 parts
Slaked lime (fresh) 50 parts
Fine sand 50 parts
Water to thick mush.

A very strong cement which stands moderate heat is the following:

2. Casein in very fine powder 1 part
Rubbed up with silicate of soda 3 parts

A strong lute for general purposes, {35} which must be used promptly
when made:

3. White of egg made into a paste with slaked lime.

A composition for soaking corks, wood, packing, etc., to render them
impervious to oil vapors, is:

Gelatine or good glue 2 parts
Glycerine 1⁠/⁠2 to 1 part
Water 6 parts
Oil of wintergreen, etc., to keep from spoiling.

X. Silicate of Oxychloride Cements.—For oil vapors, standing the
highest heat:

1. A stiff paste of silicate of soda and asbestos.

Gaskets for superheated steam, retorts, furnaces, etc.:

2. Silicate of soda and powdered glass; dry the mixture and heat.

Not so strong, however, as the following:

3. Silicate of soda 50 parts
Asbestos 15 parts
Slaked lime 10 parts

Metal Cement:

4. Silicate of soda 1 part
Oxides of metal, such
as zinc oxide; litharge,
iron oxide,
singly or mixed 1 part

Very hard and extra strong compositions:

5. Zinc oxide 2 parts
Zinc chloride 1 part
Water to make a paste.

6. Magnesium oxide 2 parts
Magnesium chloride 1 part
Water to make a paste.

XI. Flour and Starch Compositions.—

1. The well-known flaxseed poultice sets very tough, but does not stand
water or condensed steam.

2. Flour and molasses, made by making a stiff composition of the two.
This is an excellent lute to have at hand at all times for emergency
use, etc.

3. Stiff paste of flour and strong zinc-chloride solution forms a
more impervious lute, and is more permanent as a cement. This is good
for most purposes, at ordinary temperature, where it would not be in
contact with nitric-acid vapors or condensing steam.

4. A mixture of dextrine and fine sand makes a good composition, mainly
used as core compound.

XII. Miscellaneous.—

1. Litharge.
Glycerine.

Mixed to form a stiff paste, sets and becomes very hard and strong, and
is very useful for inserting glass tubes, etc., in iron or brass.

For a high heat:

2. Alumina 1 part
Sand 4 parts
Slaked lime 1 part
Borax 1⁠/⁠2 part
Water sufficient.

A class of mixtures that can be classified only according to their
intended use are core compounds.

I.—Dextrine, about 1 part
Sand, about 10 parts
With enough water to form a paste.

II.—Powdered anthracite coal, with molasses to form a stiff paste.

III.—Rosin, partly saponified by soda lye 1 part
Flour 2 parts
Sand (with sufficient water) 4 parts

(These proportions are approximate and the amount of sand can be
increased for some purposes.)

IV.—Glue, powdered 1 part
Flour 4 parts
Sand (with sufficient water) 6 parts

For some purposes the following mixture is used. It does not seem to be
a gasket or a core compound:

V.—Oats (or wheat) ground 25 parts
Glue, powdered 6 parts
Sal ammoniac 1 part

_Paper read by Samuel S. Sadtler before the Franklin Institute._

«PASTES:»

«Dextrine Pastes.»—

I.—Borax, powdered 60 parts
Dextrine, light yellow 480 parts
Glucose 50 parts
Water 420 parts

By the aid of heat, dissolve the borax in the water and add the
dextrine and glucose. Continue the heat, but do not let the mixture
boil, and stir constantly until a homogeneous solution is obtained,
from time to time renewing the water lost by evaporation with hot
water. Finally, bring up to full weight (1,000 parts) by the addition
of hot water, then strain through flannel. Prepared in this manner the
paste remains bright and clear for a long time. It has extraordinary
adhesive properties and dries very rapidly. If care is not taken to
keep the cooking temperature below the boiling point of water, the
paste is apt to become brown and to be very brittle on drying. {36}

II.—Dissolve in hot water a sufficient quantity of dextrine to bring
it to the consistency of honey. This forms a strong adhesive paste
that will keep a long time unchanged, if the water is not allowed to
evaporate. Sheets of paper may be prepared for extempore labels by
coating one side with the paste and allowing it to dry; by slightly
wetting the gummed side, the label will adhere to glass. This paste is
very useful in the office or laboratory.

III.—Pour over 1,000 parts of dextrine 450 parts of soft water and stir
the mixture for 10 minutes. After the dextrine has absorbed the water,
put the mixture over the fire, or, preferably, on a water bath, and
heat, with lively stirring for 5 minutes, or until it forms a light
milk-like liquid, on the surface of which little bubbles begin to form
and the liquid is apparently beginning to boil. Do not allow it to come
to a boil. Remove from the fire and set in a bucket of cold water to
cool off. When cold add to every 1,000 parts of the solution 51 parts
glycerine and as much salicylic acid as will stand on the tip of a
knife blade. If the solution is too thick, thin it with water that has
been boiled and cooled off again. Do not add any more glycerine or the
solution will never set.

IV.—Soften 175 parts of thick dextrine with cold water and 250 parts of
boiling water added. Boil for 5 minutes and then add 30 parts of dilute
acetic acid, 30 parts glycerine, and a drop or two of clove oil.

V.—Powder coarsely 400 parts dextrine and dissolve in 600 parts of
water. Add 20 parts glycerine and 10 parts glucose and heat to 90° C.
(195° F.).

VI.—Stir 400 parts of dextrine with water and thin the mass with 200
parts more water, 20 parts glucose, and 10 parts aluminum sulphate.
Heat the whole to 90° C. (195° F.) in the water bath until the whole
mass becomes clear and liquid.

VII.—Warm 2 parts of dextrine, 5 parts of water, 1 part of acetic acid,
1 part of alcohol together, with occasional stirring until a complete
solution is attained.

VIII.—Dissolve by the aid of heat 100 parts of builders’ glue in 200
parts of water add 2 parts of bleached shellac dissolved previously
in 50 parts of alcohol. Dissolve by the aid of heat 50 parts of
dextrine in 50 parts of water, and mix the two solutions by stirring
the second slowly into the first. Strain the mixture through a cloth
into a shallow dish and let it harden. When needed cut off a piece of
sufficient size and warm until it becomes liquid and if necessary or
advisable thin with water.

IX.—Stir up 10 parts of dextrine with sufficient water to make a thick
broth. Then, over a light fire, heat and add 25 parts of sodium water
glass.

X.—Dissolve 5 parts of dextrine in water and add 1 part of alum.

«Fastening Cork to Metal.»—In fastening cork to iron and brass, even
when these are lacquered, a good sealing wax containing shellac will
be found to serve the purpose nicely. Wax prepared with rosin is not
suitable. The cork surface is painted with the melted sealing wax.
The surface of the metal is heated with a spirit flame entirely free
from soot, until the sealing wax melts when pressed upon the metallic
surface. The wax is held in the flame until it burns, and it is then
applied to the hot surface of the metal. The cork surface painted with
sealing wax is now held in the flame, and as soon as the wax begins to
melt the cork is pressed firmly on the metallic surface bearing the wax.

«To Paste Celluloid on Wood, Tin, or Leather.»—To attach celluloid to
wood, tin, or leather, a mixture of 1 part of shellac, 1 part of spirit
of camphor, 3 to 4 parts of alcohol and spirit of camphor (90°) is well
adapted, in which 1 part of camphor is dissolved without heating in 7
parts of spirit of wine of 0.832 specific gravity, adding 2 parts of
water.

«To Paste Paper Signs on Metal or Cloth.»—A piece of gutta percha of
the same size as the label is laid under the latter and the whole is
heated. If the heating cannot be accomplished by means of a spirit lamp
the label should be ironed down under a protective cloth or paper in
the same manner as woolen goods are pressed. This method is also very
useful for attaching paper labels to minerals.

«Paste for Fastening Leather, Oilcloth, or Similar Stuff to Table
or Desk Tops, etc.»—Use the same paste for leather as for oilcloth
or other goods, but moisten the leather before applying the paste.
Prepare the paste as follows: Mix 2 1⁠/⁠4 pounds of good wheat flour
with 2 tablespoonfuls of pulverized gum arabic or powdered rosin and
2 tablespoonfuls of pulverized alum in a clean dish with water enough
to make a uniformly thick batter; set it over a slow fire and stir
continuously until the paste is uniform and free from lumps. When the
mass has become so stout that the wooden spoon or stick will stand in
it {37} upright, it is taken from the fire and placed in another dish
and covered so that no skin will form on top. When cold, the table or
desk top, etc., is covered with a thin coat of the paste, the cloth,
etc., carefully laid on and smoothed from the center toward the edges
with a rolling pin. The trimming of edges is accomplished when the
paste has dried. To smooth out the leather after pasting, a woolen
cloth is of the best service.

«To Paste Paper on Smooth Iron.»—Over a water bath dissolve 200 parts,
by weight, of gelatine in 150 parts, by weight, of water; while
stirring add 50 parts, by weight, of acetic acid, 50 parts alcohol,
and 50 parts, by weight, of pulverized alum. The spot upon which it is
desired to attach the paper must first be rubbed with a bit of fine
emery paper.

«Paste for Affixing Cloth to Metal.»—

Starch 20 parts
Sugar 10 parts
Zinc chloride 1 part
Water 100 parts

Mix the ingredients and stir until a perfectly smooth liquid results
entirely free from lumps, then warm gradually until the liquid thickens.

«To Fix Paper upon Polished Metal.»—Dissolve 400 parts, by weight, of
dextrine in 600 parts, by weight, of water; add to this 10 parts, by
weight, of glucose, and heat almost to boiling.

«Albumen Paste.»—Fresh egg albumen is recommended as a paste for
affixing labels on bottles. It is said that labels put on with this
substance, and well dried at the time, will not loosen even when
bottles are put into water and left there for some time. Albumen, dry,
is almost proof against mold or ferments. As to cost, it is but little
if any higher than gum arabic, the white of one egg being sufficient to
attach at least 100 medium-sized labels.

«Paste for Parchment Paper.»—The best agent is made by dissolving
casein in a saturated aqueous solution of borax.

«Medical Paste.»—As an adhesive agent for medicinal purposes Professor
Reihl, of Leipsic, recommends the viscous substance contained in the
white mistletoe. It is largely present in the berries and the bark
of the plant; it is called viscin, and can be produced at one-tenth
the price of caoutchouc. Solutions in benzine may be used like those
of caoutchouc without causing any irritation if applied mixed with
medicinal remedies to the skin.

«Paste That Will Not Mold.»—Mix good white flour with cold water into a
thick paste. Be sure to stir out all the lumps; then add boiling water,
stirring all the time until thoroughly cooked. To 6 quarts of this add
1⁠/⁠2 pound light brown sugar and 1⁠/⁠4 ounce corrosive sublimate,
dissolved in a little hot water. When the paste is cool add 1 drachm
oil of lavender. This paste will keep for a long time.

«Pasting Wood and Cardboard on Metal.»—In a little water dissolve
50 parts of lead acetate and 5 parts of alum. In another receptacle
dissolve 75 parts of gum arabic in 2,000 parts of water. Into this
gum-arabic solution pour 500 parts of flour, stirring constantly, and
heat gradually to the boiling point. Mingle the solution first prepared
with the second solution. It should be kept in mind that, owing to the
lead acetate, this preparation is poisonous.

«Agar Agar Paste.»—The agar agar is broken up small, wetted with water,
and exposed in an earthenware vessel to the action of ozone pumped
under pressure into the vessel from the ozonizing apparatus. About an
hour of this bleaches the agar agar and makes it freely soluble in
boiling water, when solutions far more concentrated than has hitherto
been possible can be prepared. On cooling, the solutions assume a milky
appearance, but form no lumps and are readily reliquefied by heating.
If the solution is completely evaporated, as of course happens when
the adhesive is allowed to dry after use, it leaves a firmly holding
mass which is insoluble in cold water. Among the uses to which the
preparation can be applied are the dressing of textile fabrics and
paper sizing, and the production of photographic papers, as well as the
ordinary uses of an adhesive.

«Strongly Adhesive Paste.»—Four parts glue are soaked a few hours in
15 parts cold water, and moderately heated till the solution becomes
perfectly clear, when 65 parts boiling water are added, while stirring.
In another vessel 30 parts boiled starch are previously stirred
together with 20 parts cold water, so that a thin, milky liquid without
lumps results. The boiling glue solution is poured into this while
stirring constantly, and the whole is kept boiling another 10 minutes.

«Paste for Tissue Paper.»—

(_a_) Pulverized gum arabic 2 ounces
White sugar 4 drachms
Boiling water 3 fluidounces {38}
(_b_) Common laundry starch 1 1⁠/⁠2 ounces
Cold water 3 fluidounces

Make into a batter and pour into

Boiling water 32 fluidounces

Mix (_a_) with (_b_), and keep in a wide-mouthed bottle.

«Waterproof and Acidproof Pastes.»—

I.—Chromic acid 2 1⁠/⁠2 parts
Stronger ammonia 15 parts
Sulphuric acid 1⁠/⁠2 part
Cuprammonium solution 30 parts
Fine white paper 4 parts
II.—Isinglass, a sufficient quantity
Acetic acid 1 part
Water 7 parts

Dissolve sufficient isinglass in the mixture of acetic acid and water
to make a thin mucilage.

One of the solutions is applied to the surface of one sheet of paper
and the other to the other sheet, and they are then pressed together.

III.—A fair knotting varnish free from surplus oil is by far the best
adhesive for fixing labels, especially on metal surfaces. It dries
instantly, insuring a speedy job and immediate packing, if needful,
without fear of derangement. It has great tenacity, and is not only
absolutely damp-proof itself, but is actually repellent of moisture, to
which all water pastes are subject. It costs more, but the additional
expense is often infinitesimal compared with the pleasure of a
satisfactory result.

«Balkan Paste.»—

Pale glue 4 ounces
White loaf sugar 2 ounces
Powdered starch 1 ounce
White dextrine 1⁠/⁠4 pound
Pure glycerine 3 ounces
Carbolic acid 1⁠/⁠4 ounce
Boiling water 32 ounces

Cut up the glue and steep it in 1⁠/⁠2 pint boiling water; when softened
melt in a saucepan; add sugar, starch, and dextrine, and lastly the
glycerine, in which carbolic acid has been mixed; add remainder of
water, and boil until it thickens. Pour into jars or bottles.

«Permanent Paste.»—

I.—Wheat flour 1 pound
Water, cold 1 quart
Nitric acid 4 fluidrachms
Boric acid 40 grains
Oil of cloves 20 minims

Mix the flour, boric acid, and water, then strain the mixture; add
the nitric acid, apply heat with constant stirring until the mixture
thickens; when nearly cold add the oil of cloves. This paste will have
a pleasant smell, will not attract flies, and can be thinned by the
addition of cold water as needed.

II.—Dissolve 4 ounces alum in 4 quarts hot water. When cool add as much
flour as will make it of the usual consistency; then stir into it 1⁠/⁠2
ounce powdered rosin; next add a little water in which a dozen cloves
have been steeped; then boil it until thick as mush, stirring from the
bottom all the time. Thin with warm water for use.

«Preservatives for Paste.»—Various antiseptics are employed for the
preservation of flour paste, mucilage, etc. Boric and salicylic acids,
oil of cloves, oil of sassafras, and solution of formaldehyde are among
those which have given best service. A durable starch paste is produced
by adding some borax to the water used in making it. A paste from 10
parts (weight) starch to 100 parts (weight) water with 1 per cent borax
added will keep many weeks, while without this addition it will sour
after six days. In the case of a gluing material prepared from starch
paste and joiners’ glue, borax has also demonstrated its preserving
qualities. The solution is made by mixing 10 parts (weight) starch into
a paste with water and adding 10 parts (weight) glue soaked in water to
the hot solution; the addition of 1⁠/⁠10 part (weight) of borax to the
solution will cause it to keep for weeks. It is equal to the best glue,
but should be warmed and stirred before use.

«Board-Sizing.»—A cheap sizing for rough, weather-beaten boards may be
made by dissolving shellac in sal soda and adding some heavy-bodied
pigment. This size will stick to grease spots. Linseed oil may be
added if desired. Limewater and linseed oil make a good heavy sizing,
but hard to spread. They are usually used half and half, though these
proportions may be varied somewhat.

«Rice Paste.»—Mix the rice flour with cold water, and boil it over a
gentle fire until it thickens. This paste is quite white and becomes
transparent on drying. It is very adherent and of great use for many
purposes.

«Casein Paste.»—A solution of tannin, prepared from a bark or from
commercial tannin, is precipitated with limewater, the lime being added
until the solution just turns red litmus paper blue. The supernatant
liquid is then decanted, {39} and the precipitate is dried without
artificial heat. The resulting calcium tannate is then mixed, according
to the purpose for which the adhesive is intended, with from 1 to 10
times its weight of dry casein by grinding in a mill. The adhesive
compound is soluble in water, petroleum, oils, and carbon bisulphide.
It is very strong, and is applied in the form of a paste with water.

«PASTES FOR PAPERHANGERS.»

I.—Use a cheap grade of rye or wheat flour, mix thoroughly with cold
water to about the consistency of dough, or a little thinner, being
careful to remove all lumps; stir in a tablespoonful of powdered alum
to a quart of flour, then pour in boiling water, stirring rapidly until
the flour is thoroughly cooked. Let this cool before using, and thin
with cold water.

II.—Venetian Paste.—

(_a_) 4 ounces white or fish glue
8 fluidounces cold water
(_b_) 2 fluidounces Venice turpentine
(_c_) 1 pound rye flour
16 fluidounces (1 pint) cold water
(_d_) 64 fluidounces (1⁠/⁠2 gallon) boiling water

Soak the 4 ounces of glue in the cold water for 4 hours; dissolve on
a water bath (glue pot), and while hot stir in the Venice turpentine.
Make up (_c_) into a batter free from lumps and pour into (_d_). Stir
briskly, and finally add the glue solution. This makes a very strong
paste, and it will adhere to a painted surface, owing to the Venice
turpentine in its composition.

III.—Strong Adhesive Paste.—

(_a_) 4 pounds rye flour
1⁠/⁠2 gallon cold water
(_b_) 1 1⁠/⁠2 gallons boiling water
(_c_) 2 ounces pulverized rosin

Make (_a_) into a batter free from lumps; then pour into (_b_). Boil
if necessary, and while hot stir in the pulverized rosin a little at a
time. This paste is exceedingly strong, and will stick heavy wall paper
or thin leather. If the paste be too thick, thin with a little hot
water; never thin paste with cold water.

IV.—Flour Paste.—

(_a_) 2 pounds wheat flour
32 fluidounces (1 quart) cold water
(_b_) 1 ounce alum
4 fluidounces hot water
(_c_) 96 fluidounces (1⁠/⁠2 gallon) boiling water

Work the wheat flour into a batter free from lumps with the cold water.
Dissolve the alum as designated in (_b_). Now stir in (_a_) and (_c_)
and, if necessary, continue boiling until the paste thickens into a
semitransparent mucilage, after which stir in solution (_b_). The above
makes a very fine paste for wall paper.

V.—Elastic or Pliable Paste.—

(_a_) 4 ounces common starch
2 ounces white dextrine
10 fluidounces cold water

(_b_) 1 ounce borax
3 fluidounces glycerine
64 fluidounces (1⁠/⁠2 gallon) boiling water

Beat to a batter the ingredients of (_a_). Dissolve the borax in the
boiling water; then add the glycerine, after which pour (_a_) into
solution (_b_). Stir until it becomes translucent. This paste will not
crack, and, being very pliable, is used for paper, cloth, leather, and
other material where flexibility is required.

VI.—A paste with which wall paper can be attached to wood or masonry,
adhering to it firmly in spite of dampness, is prepared, as usual, of
rye flour, to which, however, are added, after the boiling, 8 1⁠/⁠3
parts, by weight, of good linseed-oil varnish and 8 1⁠/⁠3 parts, by
weight, of turpentine to every 500 parts, by weight.

VII.—Paste for Wall Paper.—Soak 18 pounds of bolus (bole) in water,
after it has been beaten into small fragments, and pour off the
supernatant water. Boil 10 ounces of glue into glue water, mix it
well with the softened bolus and 2 pounds plaster of Paris and strain
through a sieve by means of a brush. Thin the mass with water to the
consistency of a thin paste. The paste is now ready for use. It is not
only much cheaper than other varieties, but has the advantage over them
of adhering better to whitewashed walls, and especially such as have
been repeatedly coated over the old coatings which were not thoroughly
removed. For hanging fine wall paper this paste is less commendable, as
it forms a white color, with which the paper might easily become soiled
if great care is not exercised in applying it. If the fine wall paper
is mounted on ground paper, however, it can be recommended for pasting
the ground paper on the wall.

«LABEL PASTES:»

«Pastes to Affix Labels to Tin.»—Labels separate from tin because the
paste becomes too dry. Some moisture is presumably always present; but
more is required to cause continued adhesion in the case of tin than
where the container is of {40} glass. Paste may be kept moist by the
addition of calcium chloride, which is strongly hygroscopic, or of
glycerine.

The following formulas for pastes of the type indicated were proposed
by Leo Eliel:

I.—Tragacanth 1 ounce
Acacia 4 ounces
Thymol 14 grains
Glycerine 4 ounces
Water, sufficient to make 2 pints

Dissolve the gums in 1 pint of water, strain, and add the glycerine, in
which the thymol is suspended; shake well and add sufficient water to
make 2 pints. This separates on standing, but a single shake mixes it
sufficiently for use.

II.—Rye flour 8 ounces
Powdered acacia 1 ounce
Glycerine 2 ounces
Oil of cloves 40 drops

Rub the rye flour and acacia to a smooth paste with 8 ounces of cold
water; strain through cheese cloth, and pour into 1 pint of boiling
water, and continue the heat until as thick as desired. When nearly
cold add the glycerine and oil of cloves.

III.—Rye flour 5 parts
Venice turpentine 1 part
Liquid glue, a sufficient quantity

Rub up the flour with the turpentine and then add sufficient freshly
prepared glue (glue or gelatine dissolved in water) to make a stiff
paste. This paste dries slowly.

IV.—Dextrine 2 parts
Acetic acid 1 part
Water 5 parts
Alcohol, 95 per cent. 1 part

Dissolve the dextrine and acetic acid in water by heating together in
the water bath, and to the solution add the alcohol.

V.—Dextrine 3 pounds
Borax 2 ounces
Glucose 5 drachms
Water 3 pints 2 ounces

Dissolve the borax in the water by warming, then add the dextrine and
glucose, and continue to heat gently until dissolved.

Another variety is made by dissolving a cheap Ghatti gum in limewater,
but it keeps badly.

VI.—Add tartaric acid to thick flour paste. The paste is to be boiled
until quite thick, and the acid, previously dissolved in a little
water, is added, the proportion being about 2 ounces to the pint of
paste.

VII.—Gum arabic, 50 parts; glycerine, 10 parts; water, 30 parts; liq.
Stibii chlorat., 2 parts.

VIII.—Boil rye flour and strong glue water into a mass to which are
added, for 1,000 parts, good linseed-oil varnish 30 parts and oil of
turpentine 30 parts. This mixture furnishes a gluing agent which, it
is claimed, even renders the labels proof against being loosened by
moisture.

IX.—Pour 140 parts of distilled cold water over 100 parts of gum arabic
in a wide-necked bottle and dissolve by frequent shaking. To the
solution, which is ready after standing for about 3 days, add 10 parts
of glycerine; later, 20 parts of diluted acetic acid, and finally 6
parts of aluminum sulphate, then straining it through a fine-hair sieve.

X.—Good glue is said to be obtained by dissolving 1 part of powdered
sugar in 4 parts of soda water glass.

XI.—A glue for bottle labels is prepared by dissolving borax in water;
soak glue in this solution and dissolve the glue by boiling. Carefully
drop as much acetic acid into the solution as will allow it to remain
thin on cooling. Labels affixed with this agent adhere firmly and do
not become moldy in damp cellars.

XII.—Dissolve some isinglass in acetic acid and brush the labels over
with it. There will be no cause to complain of their coming off, nor
of striking through the paper. Take a wide-mouthed bottle, fill about
two-thirds with commercial acetic acid, and put in as much isinglass as
the liquid will hold, and set aside in a warm place until completely
dissolved. When cold it should form a jelly. To use it place the bottle
in hot water. The cork should be well-fitting and smeared with vaseline
or melted paraffine.

«How to Paste Labels on Tin.»—Brush over the entire back of the label
with a flour paste, fold the label loosely by sticking both ends
together without creasing the center, and throw to one side until this
process has been gone through with the whole lot. Then unfold each
label and place it on the can in the regular manner. The paste ought
not to be thicker than maple syrup. When of this consistency it soaks
through the label and makes it pliable and in a condition to be easily
rubbed into position. If the paste is too thick it dries quickly, and
does not soak through the label sufficiently. After the labels have
been placed upon the cans the latter must be {41} kept apart until dry.
In putting the paste upon the labels in the first place, follow the
method of placing the dry labels over one another, back sides up, with
the edge of each just protruding over the edge of the one beneath it,
so that the fingers may easily grasp the label after the pasting has
been done.

«Druggists’ Label Paste.»—This paste, when carefully made, is an
admirable one for label use, and a very little will go a long way:

Wheat flour 4 ounces
Nitric acid 1 drachm
Boric acid 10 grains
Oil of cloves 5 drops
Carbolic acid 1⁠/⁠2 drachm

Stir flour and water together, mixing thoroughly, and add the other
ingredients. After the stuff is well mixed, heat it, watching very
carefully and removing the instant it stiffens.

«To Attach Glass Labels to Bottles.»—Melt together 1 part of rosin and
2 parts of yellow wax, and use while warm.

«Photographic Mountants (see also Photography).»—Owing to the nature
of the different papers used for printing photographs, it is a
matter of extreme importance to use a mountant that shall not set up
decomposition in the coating of the print. For example, a mountant that
exhibits acidity or alkalinity is injurious with most varieties of
paper; and in photography the following formulas for pastes, mucilages,
etc., have therefore been selected with regard to their absolute
immunity from setting up decomposition in the print or changing its
tone in any way. One of the usual mountants is rice starch or else
rice water. The latter is boiled to a thick jelly, strained, and the
strained mass used as an agglutinant for attaching photographic prints
to the mounts. There is nothing of an injurious nature whatever in this
mountant, neither is there in a mucilage made with gum dragon.

This gum (also called gum tragacanth) is usually in the form of curls
(i.e., leaf gum), which take a long time to properly dissolve in
water—several weeks, in fact—but during the past few years there has
been put on the market a powdered gum dragon which does not occupy so
many days in dissolving. To make a mucilage from gum dragon a very
large volume of water is required. For example, 1 ounce of the gum,
either leaf or powder, will swell up and convert 1 gallon of water into
a thickish mucilage in the course of 2 or 3 weeks. Only cold water must
be used, and before using the mucilage, all whitish lumps (which are
particles of undissolved gum) should be picked out or else the mucilage
strained. The time of solution can be considerably shortened (to a few
hours) by acidifying the water in which the gum is placed with a little
sulphuric or oxalic acid; but as the resultant mucilage would contain
traces of their presence, such acids are not permissible when the
gum-dragon mucilage is to be used for mounting photographs.

Glycerine and gum arabic make a very good adhesive of a fluid nature
suited to mounting photographs; and although glycerine is hygroscopic
by itself, such tendency to absorb moisture is checked by the reverse
nature of the gum arabic; consequently an ideal fluid mucilage is
produced. The proportions of the several ingredients are these:

Gum arabic, genuine (gum acacia, not Bassora gum) 4 ounces
Boiling water 12 ounces
Glycerine, pure 1 ounce

First dissolve the gum in the water, and then stir in the glycerine,
and allow all _débris_ from the gum to deposit before using. The
following adhesive compound is also one that is free from chemical
reactions, and is suited for photographic purposes:

Water 2 pints
Gum dragon, powdered 1 ounce
Gum arabic, genuine 4 ounces
Glycerine 4 ounces

Mix the gum arabic with half the water, and in the remainder of the
water dissolve the gum dragon. When both solids are dissolved, mix them
together, and then stir in the glycerine.

The following paste will be found a useful mountant:

Gum arabic, genuine 1 ounce
Rice starch 1 ounce
White sugar 4 ounces
Water, q. s.

Dissolve the gum in just sufficient water to completely dissolve it,
then add the sugar, and when that has completely dissolved stir in the
starch paste, and then boil the mixture until the starch is properly
cooked.

A very strong, stiff paste for fastening cardboard mounts to frames,
wood, and other materials is prepared by making a bowl of starch
paste in the usual way, and then adding 1 ounce of Venice turpentine
per pound of paste, and {42} boiling and stirring the mixture until
the thick turpentine has become well incorporated. Venice turpentine
stirred into flour paste and boiled will also be found a very
adhesive cement for fastening cardboard, strawboard, leatherette, and
skiver leather to wood or metal; but owing to the resinous nature
of the Venice turpentine, such pastes are not suitable for mounting
photographic prints. The following half-dozen compounds are suitable
mountants to use with silver prints:

Alcohol, absolute 10 ounces
Gelatine, good 1 ounce
Glycerine 1⁠/⁠2 to 1 ounce

Soak the gelatine in water for an hour or two until it is completely
softened; take the gelatine out of the water, and allow it to drain,
and put it into a bottle and pour alcohol over it; add the glycerine
(if the gelatine is soft, use only 1⁠/⁠2 ounce; if the gelatine is
hard, use 1 ounce of the glycerine), then melt the gelatine by standing
the bottle in a vessel of hot water, and shake up very well. For use,
remelt by heat. The alcohol prevents the prints from stretching or
cockling, as they are apt to, under the influence of the gelatine.

In the following compound, however, only sufficient alcohol is used to
serve as an antiseptic, and prevent the agglutinant from decomposing:
Dissolve 4 ounces of photographic gelatine in 16 ounces of water (first
soaking the gelatine therein for an hour or two until it is completely
softened), then remove the gelatine from the water, allow it to drain,
and put it into the bottle, and pour the alcohol over it, and put in
the glycerine (if the gelatine is soft, use only 1⁠/⁠2 ounce; if the
gelatine is hard, use 1 ounce of the glycerine), then melt the gelatine
by standing the bottle in a vessel of hot water, and shake up well and
mix thoroughly. For use, remelt by heat. The alcohol prevents the print
from stretching or cockling up under the influence of the gelatine.

The following paste agglutinant is one that is very permanent and
useful for all purposes required in a photographic studio: Take 5 pints
of water, 10 ounces of arrowroot, 1 ounce of gelatine, and a 1⁠/⁠2 pint
(10 fluidounces) of alcohol, and proceed to combine them as follows:
Make arrowroot into a thick cream with a little of the water, and in
the remainder of the water soak the gelatine for a few hours, after
which melt the gelatine in the water by heating it, add the arrowroot
paste, and bring the mixture to the boil and allow to boil for 4 or 5
minutes, then allow to cool, and mix in the alcohol, adding a few drops
of oil of cloves.

Perhaps one of the most useful compounds for photographic purposes is
that prepared as follows: Soak 4 ounces of hard gelatine in 15 ounces
of water for a few hours, then melt the gelatine by heating it in a
glue pot until the solution is quite clear and free from lumps, stir in
65 fluidounces of cold water so that it is free from lumps, and pour in
the boiling-hot solution of gelatine and continue stirring, and if the
starch is not completely cooked, boil up the mixture for a few minutes
until it “blows,” being careful to keep it well stirred so as not to
burn; when cold add a few drops of carbolic acid or some essential oil
as an antiseptic to prevent the compound from decomposing or becoming
sour.

A useful photographic mucilage, which is very liquid, is obtained
by mixing equal bulks of gum-arabic and gum-dragon mucilages of the
same consistence. The mixture of these mucilages will be considerably
thinner than either of them when alone.

As an agglutinant for general use in the studio, the following is
recommended: Dissolve 2 ounces of gum arabic in 5 ounces of water,
and for every 250 parts of the mucilage add 20 parts of a solution of
sulphate of aluminum, prepared by dissolving 1 part of the sulphate
in 20 parts of water (common alum should not be used, only the pure
aluminum sulphate, because common alum is a mixture of sulphates, and
usually contaminated with iron salts). The addition of the sulphate
solution to the gum mucilage renders the latter less hygroscopic, and
practically waterproof, besides being very adhesive to any materials,
particularly those exhibiting a smooth surface.

«MUCILAGES:»

«For Affixing Labels to Glass and Other Objects.»—I.—The mucilage is
made by simply pouring over the gum enough water to a little more
than cover it, and then, as the gum swells, adding more water from
time to time in small portions, until the mucilage is brought to such
consistency that it may be easily spread with the brush. The mucilage
keeps fairly well without the addition of any antiseptic.

II.—Tragacanth 1 ounce
Acacia 4 ounces
Thymol 14 grains
Glycerine 4 ounces
Water, sufficient to make 2 pints

{43}

Dissolve the gums in 1 pint of water, strain and add the glycerine, in
which the thymol is suspended; shake well and add sufficient water to
make 2 pints. This separates on standing, but a single shake mixes it
sufficiently for use.

III.—Rye flour 8 ounces
Powdered acacia 1 ounce
Glycerine 2 ounces
Oil of cloves 40 drops
Water, a sufficient quantity.

Rub the rye flour and the acacia to a smooth paste with 8 ounces of
cold water; strain through cheese cloth, and pour into 1 pint of
boiling water and continue the heat until as thick as desired. When
nearly cold add the glycerine and oil of cloves.

IV.—One part, by weight, of tragacanth, when mixed with 95-per-cent
alcohol to form 4 fluidounces, forms a liquid in which a portion of
the tragacanth is dissolved and the remainder suspended; this remains
permanently fluid, never deteriorates, and can be used in place of the
present mucilage; 4 to 8 minims to each ounce of mixture is sufficient
to suspend any of the insoluble substances usually given in mixtures.

V.—To 250 parts of gum-arabic mucilage add 20 parts of water and 2
parts of sulphate of alumina and heat until dissolved.

VI.—Dissolve 1⁠/⁠2 pound gum tragacanth, powdered, 1⁠/⁠4 pound gum
arabic, powdered, cold water to the desired consistency, and add 40
drops carbolic acid.

«Mucilage of Acacia.»—Put the gum, which should be of the best kind,
in a flask the size of which should be large enough to contain the
mucilage with about one-fifth of its space to spare (i. e., the product
should fill it about four-fifths full). Now tare, and wash the gum with
distilled water, letting the latter drain away as much as possible
before proceeding further. Add the requisite quantity of distilled
water slowly, which, however, should first have added to it about 10
per cent of limewater. Now cork the flask, and lay it, without shaking,
horizontally in a cool place and let it remain quietly for about 3
hours, then give it a half turn to the right without disturbing its
horizontal position. Repeat this operation three or four times during
the day, and keep it up until the gum is completely dissolved (which
will not be until the fourth day probably), then strain through a thin
cloth previously wet with distilled water, avoiding, in so doing, the
formation of foam or bubbles. This precaution should also be observed
in decantation of the percolate into smaller bottles provided with
paraffine corks. The small amount of limewater, as will be understood,
is added to the solvent water in order to prevent the action of free
acid.

«Commercial Mucilage.»—Dissolve 1⁠/⁠2 pound white glue in equal parts
water and strong vinegar, and add 1⁠/⁠4 as much alcohol and 1⁠/⁠2 ounce
alum dissolved in a little water. To proceed, first get good glue and
soak in cold water until it swells and softens. Use pale vinegar. Pour
off the cold water, then melt the glue to a thick paste in hot water,
and add the vinegar hot. When a little cool add the alcohol and alum
water.

«To Render Gum Arabic More Adhesive.»—I.—Add crystallized aluminum
sulphate in the proportion of 2 dissolved in 20 parts of water to 250
parts of concentrated gum solution (75 parts of gum in 175 parts of
water).

II.—Add to 250 parts of concentrated gum solution (2 parts of gum in 5
parts of water) 2 parts of crystallized aluminum sulphate dissolved in
20 parts of water. This mixture glues even unsized paper, pasteboard
on pasteboard, wood on wood, glass, porcelain, and other substances on
which labels frequently do not adhere well.

«Envelope Gum.»—The gum used by the United States Government on postage
stamps is probably one of the best that could be used not only for
envelopes but for labels as well. It will stick to almost any surface.
Its composition is said to be the following:

Gum arabic 1 part
Starch 1 part
Sugar 4 parts
Water, sufficient to give the desired consistency.

The gum arabic is first dissolved in some water, the sugar added, then
the starch, after which the mixture is boiled for a few minutes in
order to dissolve the starch, after which it is thinned down to the
desired consistency.

Cheaper envelope gums can be made by substituting dextrine for the gum
arabic, glucose for the sugar, and adding boric acid to preserve and
help stiffen it.

«Mucilage to Make Wood and Pasteboard Adhere to Metals.»—Dissolve 50
parts, by weight, of lead acetate together with 5 parts, by weight,
of alum in a little water. Make a separate solution of 75 parts, by
weight, of gum arabic in 2,000 parts, by weight, of water, stir in
this 500 {44} parts, by weight, of flour, and heat slowly to boiling,
stirring the while. Let it cool somewhat, and mix with it the solution
containing the lead acetate and alum, stirring them well together.

«Preservation of Gum Solution.»—Put a small piece of camphor in the
mucilage bottle. Camphor vapors are generated which kill all the
bacterial germs that have entered the bottle. The gum maintains its
adhesiveness to the last drop.

ADULTERANTS IN FOODS: See Foods.

ADUROL DEVELOPER: See Photography.

ÆSCO-QUININE: See Horse Chestnut.

AGAR AGAR PASTE: See Adhesives.

«AGATE, BUTTONS OF ARTIFICIAL.»

Prepare a mixture or frit of 33 parts of quartz sand, 65 parts calcium
phosphate, and 2 parts of potash. The frit, which has been reduced by
heat to the fusing point, is finely ground, intimately mingled with a
small quantity of kaolin and pressed in molds which yield button-shaped
masses. These masses, after having been fired, are given a transparent
glaze by any of the well-known processes.

AGATE (IMITATION): See Gems, Artificial.

AGING OF SILK: See Silk.

AGING, SILVER AND GOLD: See Plating.

«AIR BATH.»

This air bath is employed in cases in which, upon drying or heating
substances, acid vapors arise because the walls of the bath are not
attacked by them. For the production of the drying apparatus take a
flask with the bottom burst off or a bell jar tubulated above. This
is placed either upon a sand bath or upon asbestos paper, previously
laid upon a piece of sheet iron. The sand bath or the sheet iron is
put on a tripod, so that it can be heated by means of a burner placed
underneath. The substance to be dried is placed in a glass or porcelain
dish, which is put under the bell jar, and if desired the drying dish
may be hung on the tripod. For regulating the temperature the tubulure
of the jar is closed with a pierced cork, through whose aperture the
thermometer is thrust. In order to permit the vapors to escape, the
cork is grooved lengthwise along the periphery.

AIR BUBBLES IN GELATINE: See Gelatine.

AIR, EXCLUSION OF, FROM SOLUTIONS: See Photography.

«AIR-PURIFYING.»

«Ozonatine» is a fragrant air-purifying preparation consisting of
dextrogyrate turpentine oil scented with slight quantities of fragrant
oils.

ALABASTER CLEANING: See Cleaning Preparations and Methods.

ALBATA METAL: See Alloys.

«ALBUMEN IN URINE, DETECTION OF.»

Patein (_Pharm. Zeit._) recommends the following test for albumen in
urine: Dissolve 250 grams of citric acid in a sufficient quantity of
water, add enough ammonia to neutralize, then 50 grams of alcohol,
and finally enough water to make 1 liter. To the acid (or acidulated)
urine, one-tenth its volume of the ammonium-citrate solution made
as above is added, and the whole heated in the usual manner. The
appearance of the faintest turbidity is said to indicate with positive
certainty the presence of albumen.

ALBUMEN PAPER: See Photography.

ALBUMEN PASTE: See Adhesives.

«Alcohol»

After the manuscript of this book was ready for the press, Congress
passed the bill which has since become a law, whereby the prohibitive
tax on industrial or denatured alcohol is removed. So important is this
legislative measure that the Editor has deemed it wise to insert an
article on the sources of alcohol and the manufacture of alcohol from
farm products. Because the first portion of the book was in type when
this step was decided upon, the Editor was compelled to relegate to a
later page a monograph which should properly have appeared here. The
reader will find the matter on alcohol referred to under the heading
{45} “Spirit”; likewise methods of denaturing and a list of denaturants.

ALCOHOL, DILUTION OF: See Tables.

«Alcohol, Tests for Absolute.»—The committee for the compilation of the
German Arzneibuch established the following tests for the determination
of absolute alcohol:

Absolute alcohol is a clear, colorless, volatile, readily imflammable
liquid which burns with a faintly luminous flame. Absolute alcohol has
a peculiar odor, a burning taste, and does not affect litmus paper.
Boiling point, 78.50. Specific gravity, 0.795 to 0.797. One hundred
parts contain 99.7 to 99.4 parts, by volume, or 99.6 to 99.0 parts, by
weight, of alcohol.

Absolute alcohol should have no foreign smell and should mix with water
without cloudiness.

After the admixture of 5 drops of silver-nitrate solution, 10 cubic
centimeters of absolute alcohol should not become turbid or colored
even on heating.

A mixture of 10 cubic centimeters of absolute alcohol and 0.2 cubic
centimeter of potash lye evaporated down to 1 cubic centimeter should
not exhibit an odor of fusel oil after supersaturation with dilute
sulphuric acid.

Five cubic centimeters of sulphuric acid, carefully covered, in a
test tube, with a stratum of 5 cubic centimeters of absolute alcohol,
should not form a rose-colored zone at the surface of contact, even on
standing for some time.

The red color of a mixture of 10 cubic centimeters of absolute alcohol
and 1 cubic centimeter of potassium-permanganate solution should not
pass into yellow before 20 minutes.

Absolute alcohol should not be dyed by hydrogen sulphide water or by
aqueous ammonia.

Five cubic centimeters of absolute alcohol should not leave behind a
weighable residue after evaporation on water bath.

«Absolute Alcohol.»—If gelatine be suspended in ordinary alcohol
it will absorb the water, but as it is insoluble in alcohol, that
substance will remain behind, and thus nearly absolute alcohol will be
obtained without distillation.

«Perfumed Denaturized Alcohol.»—

East India lemon oil 1,250 parts
Mirbane oil 1,000 parts
Cassia oil 50 parts
Clove oil 75 parts
Lemon oil 100 parts
Amyl acetate 500 parts
Spirit (95 per cent) 7,000 parts

Dissolve the oils in the spirit and add the amyl acetate. The mixture
serves for destroying the bad odor of denaturized spirit in distilling.
Use 50 parts of the perfume per 1,000 parts of spirit.

«Solid Alcohol.»—I.—Heat 1,000 parts of denaturized alcohol (90 per
cent) in a flask of double the capacity on the water bath to about
140° F., and then mix with 28 to 30 parts of well-dried, rasped
Venetian soap and 2 parts of gum lac. After repeated shaking, complete
dissolution will take place. The solution is put, while still warm,
into metallic vessels, closing them up at once and allowing the mixture
to cool therein. The admixture of gum lac effects a better preservation
and also prevents the evaporation of the alcohol. On lighting the solid
spirit the soap remains behind.

II.—Smaragdine is a trade name for solidified alcohol. It consists of
alcohol and gun cotton, colored with malachite green. It appears in the
market in the form of small cubes.

«Alcohol in Fermented Beers.»—Experience has shown that 1⁠/⁠4 pound of
sugar to 1 gallon of water yields about 2 per cent of proof spirit,
or about 1 per cent of absolute alcohol. Beyond this amount it is not
safe to go, if the legal limit is to be observed, yet a ginger beer
brewed with 1⁠/⁠4 pound per gallon of sugar would be a very wishy-washy
compound, and there is little doubt that a much larger quantity is
generally used. The more sugar that is used—up to 1 1⁠/⁠2 or 1 1⁠/⁠4
pounds per gallon—the better the drink will be and the more customers
will relish it; but it will be as “strong” as lager and contain perhaps
5 per cent of alcohol, which will make it anything but a “temperance”
drink. Any maker who is using as much as even 1⁠/⁠2 pound of sugar per
gallon is bound to get more spirit than the law allows. Meanwhile it is
scarcely accurate to term ginger beers, etc., non-alcoholic.

«Alcohol Deodorizer.»—

Alcohol 160 ounces
Powdered quicklime 300 grains
Powdered alum 150 grains
Spirit of nitrous ether 1 1⁠/⁠4 drachms

Mix the lime and alum intimately by trituration; add the alcohol and
shake well; then add the spirit of nitrous ether; set aside for 7 days
and filter through animal charcoal.

«Denaturized Alcohol.»—There are two general classes or degrees of
denaturizing, viz., the “complete” and the “incomplete,” according
to the purpose for {46} which the alcohol so denaturized is to be
ultimately used.

I.—Complete denaturization by the German system is accomplished by the
addition to every 100 liters (equal to 26 1⁠/⁠2 gallons) of spirits:

(_a_) Two and one-half liters of the “standard” denaturizer, made of 4
parts of wood alcohol, 1 part of pyridine (a nitrogenous base obtained
by distilling bone oil or coal tar), with the addition of 50 grams to
each liter of oil of lavender or rosemary.

(_b_) One and one-fourth liters of the above “standard” and 2 liters of
benzol with every 100 liters of alcohol.

II.—Incomplete denaturization—i. e., sufficient to prevent alcohol
from being drunk, but not to disqualify it from use for various
special purposes, for which the wholly denaturized spirits would be
unavailable—is accomplished by several methods as follows, the quantity
and nature of each substance given being the prescribed dose for each
100 liters (26 1⁠/⁠2 gallons) of spirits:

(_c_) Five liters of wood alcohol or 1⁠/⁠2 liter of pyridine.

(_d_) Twenty liters of solution of shellac, containing 1 part gum to
2 parts alcohol of 90-per-cent purity. Alcohol for the manufacture of
celluloid and pegamoid is denaturized.

(_e_) By the addition of 1 kilogram of camphor or 2 liters oil of
turpentine or 1⁠/⁠2 liter benzol to each 100 liters of spirits. Alcohol
to be used in the manufacture of ethers, aldehyde, agaricin, white
lead, bromo-silver gelatines, photographic papers and plates, electrode
plates, collodion, salicylic acid and salts, aniline chemistry, and a
great number of other purposes, is denaturized by the addition of—

(_f_) Ten liters sulphuric ether, or 1 part of benzol, or 1⁠/⁠2 part
oil of turpentine, or 0.025 part of animal oil.

For the manufacture of varnishes and inks alcohol is denaturized by the
addition of oil of turpentine or animal oil, and for the production of
soda soaps by the addition of 1 kilogram of castor oil. Alcohol for the
production of lanolin is prepared by adding 5 liters of benzine to each
hectoliter of spirits.

«ALE.»

The ale of the modern brewer is manufactured in several varieties,
which are determined by the wants of the consumer and the particular
market for which it is intended. Thus, the finer kinds of Burton, East
India, Bavarian, and other like ales, having undergone a thorough
fermentation, contain only a small quantity of undecomposed sugar and
gum, varying from 1 to 5 per cent. Some of these are highly “hopped” or
“bittered,” the further to promote their preservation during transit
and change of temperature. Mild or sweet ales, on the contrary, are
less accentuated by lengthened fermentation, and abound in saccharine
and gummy matter. They are, therefore, more nutritious, though less
intoxicating, than those previously referred to.

In brewing the finer kinds of ales, pale malt and the best hops of the
current season’s growth are always employed; and when it is desired to
produce a liquor possessing little color, very great attention is paid
to their selection. With the same object, the boiling is conducted with
more than the usual precautions, and the fermentation is carried on
at a somewhat lower temperature than that commonly allowed for other
varieties of beer. For ordinary ale, intended for immediate use, the
malt may be all pale; but, if the liquor be brewed for keeping, and
in warm weather, when a slight color is not objectionable, one-fifth,
or even one-fourth of amber malt may be advantageously employed. From
4 1⁠/⁠2 to 6 pounds of hops is the quantity commonly used to the
one-fourth of malt, for ordinary ales; and 7 pounds to 10 pounds for
“keeping” ales. The proportions, however, must greatly depend on the
intended quality and description of the brewing and the period that
will be allowed for its maturation.

The stronger varieties of ale usually contain from 6 to 8 per cent
of “absolute alcohol”; ordinary strong ale, 4 1⁠/⁠2 to 6 per cent;
mild ale, 3 to 4 percent; and table ale, 1 to 1 1⁠/⁠2 per cent (each
by volume); together with some undecomposed saccharine, gummy, and
extractive matter, the bitter and narcotic principles of the hop, some
acetic acid formed by the oxidation of the alcohol, and very small and
variable quantities of mineral and saline matter.

Ordinary ale-wort (preferably pale), sufficient to produce 1 barrel,
is slowly boiled with about 3 handfuls of hops, and 12 to 14 pounds of
crushed groats, until the whole of the soluble matter of the latter
is extracted. The resulting liquor, after being run through a coarse
strainer and become lukewarm, is fermented with 2 or 3 pints of yeast;
and, as soon as the fermentation is at its height, is either closely
bunged up for draft or is at once put into strong stoneware bottles,
which are then well corked and wired.

White ale is said to be very nutritious, though apt to prove laxative
to those {47} unaccustomed to its use. It is drunk in a state of
effervescence or lively fermentation; the glass or cup containing it
being kept in constant motion, when removed from the mouth, until the
whole is consumed, in order that the thicker portion may not subside to
the bottom.

ALE, GINGER: See Beverages.

ALFENIDE METAL: See Alloys.

ALKALI, HOW TO DETECT: See Soaps.

ALKALOIDS, ANTIDOTES TO: See Atropine.

«Alloys»

No general rules can be given for alloying metals. Alloys differing
greatly in fusibility are commonly made by adding the more fusible
ones, either in the melted state or in small portions at a time, to
the other melted or heated to the lowest possible temperature at which
a perfect union will take place between them. The mixture is usually
effected under a flux, or some material that will promote liquefaction
and prevent volatilization and unnecessary exposure to the air. Thus,
in melting lead and tin together for solder, rosin or tallow is thrown
upon the surface is rubbed with sal ammoniac; and in combining some
metals, powdered charcoal is used for the same purpose. Mercury or
quicksilver combines with many metals in the cold, forming AMALGAMS, or
easily fusible alloys (q. v.).

Alloys generally possess characteristics unshared by their component
metals. Thus, copper and zinc form brass, which has a different
density, hardness, and color from either of its constituents. Whether
the metals tend to unite in atomic proportions or in any definite ratio
is still undetermined. The evidence afforded by the natural alloys
of gold and silver, and by the phenomena accompanying the cooling of
several alloys from the state of fusion, goes far to prove that such
is the case (Rudberg). The subject is, however, one of considerable
difficulty, as metals and metallic compounds are generally soluble
in each other, and unite by simple fusion and contact. That they do
not combine indifferently with each other, but exercise a species of
elective affinity not dissimilar to other bodies, is clearly shown
by the homogeneity and superior quality of many alloys in which the
constituent metals are in atomic proportion. The variation of the
specific gravity and melting points of alloys from the mean of those
of their component metals also affords strong evidence of a chemical
change having taken place. Thus, alloys generally melt at lower
temperatures than their separate metals. They also usually possess more
tenacity and hardness than the mean of their constituents.

Matthiessen found that when weights are suspended to spirals of
hard-drawn wire made of copper, gold, or platinum, they become nearly
straightened when stretched by a moderate weight; but wires of equal
dimensions composed of copper-tin (12 per cent of tin), silver-platinum
(36 per cent of platinum), and gold-copper (84 per cent of copper)
scarcely undergo any permanent change in form when subjected to tension
by the same weight.

The same chemist gives the following approximate results upon the
tenacity of certain metals and wires hard-drawn through the same gauge
(No. 23):

Pounds
Copper, breaking strain 25–30
Tin, breaking strain under 7
Lead, breaking strain under 7
Tin-lead (20% lead) about 7
Tin-copper (12% copper) about 7
Copper-tin (12% tin) about 80–90
Gold (12% tin) 20–25
Gold-copper (8.4% copper) 70–75
Silver (8.4% copper) 45–50
Platinum (8.4% copper) 45–50
Silver-platinum (30% platinum) 75–80

On the other hand, the malleability, ductility, and power of resisting
oxygen of alloys is generally diminished. The alloy formed of two
brittle metals is always brittle; that of a brittle and a ductile
metal, generally so; and even two ductile metals sometimes unite to
form a brittle compound. The alloys formed of metals having different
fusing points are usually malleable while cold and brittle while hot.
The action of the air on alloys is generally less than on their simple
metals, unless the former are heated. A mixture of 1 part of tin and 3
parts of lead is scarcely acted on at common temperatures; but at a red
heat it readily takes fire, and continues to burn for some time like
a piece of bad turf. In like manner, a mixture of tin and zinc, when
strongly heated, decomposes both moist air and steam with rapidity.

The specific gravity of alloys is rarely {48} the arithmetical mean
of that of their constituents, as commonly taught; and in many cases
considerable condensation or expansion occurs. When there is a strong
affinity between two metals, the density of their alloy is generally
greater than the calculated mean; and vice versa, as may be seen in the
following table:

ALLOYS HAVING A DENSITY
Greater than the Mean of their Constituents:

Copper and bismuth,
Copper and palladium,
Copper and tin,
Copper and zinc,
Gold and antimony,
Gold and bismuth,
Gold and cobalt,
Gold and tin,
Gold and zinc,
Lead and antimony,
Palladium and bismuth,
Silver and antimony,
Silver and bismuth,
Silver and lead,
Silver and tin,
Silver and zinc.

Less than the Mean of their Constituents:

Gold and copper,
Gold and iridium,
Gold and iron,
Gold and lead,
Gold and nickel,
Gold and silver,
Iron and antimony,
Iron and bismuth,
Iron and lead,
Nickel and arsenic,
Silver and copper,
Tin and antimony,
Tin and lead,
Tin and palladium,
Zinc and antimony.

«Compounding Alloys.»—Considerable experience is necessary to insure
success in compounding alloys, especially when the metals employed vary
greatly in fusibility and volatility. The following are rules supplied
by an experienced workman:

1. Melt the least fusible, oxidizable, and volatile first, and then add
the others heated to their point of fusion or near it. Thus, if it is
desired to make an alloy of exactly 1 part of copper and 3 of zinc, it
will be impossible to do so by putting proportions of the metals in a
crucible and exposing the whole to heat. Much of the zinc would fly off
in vapor before the copper was melted. First, melt the copper and add
the zinc, which has been melted in another crucible. The zinc should be
in excess, as some of it will be lost anyway.

2. Some alloys, as copper and zinc, copper and arsenic, may be formed
by exposing heated plates of the least fusible metal to the vapor of
the other. In making brass in the large way, thin plates of copper are
dissolved, as it were, in melted zinc until the proper proportions have
been obtained.

3. The surface of all oxidizable metals should be covered with some
protecting agent, as tallow for very fusible ones, rosin for lead and
tin, charcoal for zinc, copper, etc.

4. Stir the metal before casting and if possible, when casting, with a
whitewood stick; this is much better for the purpose than an iron rod.

5. If possible, add a small portion of old alloy to the new. If
the alloy is required to make sharp castings and strength is not a
very great object, the proportion of old alloy to the new should be
increased. In all cases a new or thoroughly well-cleansed crucible
should be used.

To obtain metals and metallic alloys from their compounds, such as
oxides, sulphides, chlorides, etc., a process lately patented makes use
of the reducing qualities of aluminum or its alloys with magnesium. The
finely powdered material (e. g., chromic oxide) is placed in a crucible
mixed with aluminum oxide. The mixture is set afire by means of a
soldering pipe or a burning magnesium wire, and the desired reaction
takes place. For igniting, one may also employ with advantage a special
priming cartridge consisting of pulverized aluminum to which a little
magnesium may be mixed, and peroxide of magnesia, which is shaped into
balls and lighted with a magnesium wire. By suitable additions to the
pulverized mixture, alloys containing aluminum, magnetism, chromium,
manganese, copper, iron, boron, silicic acid, etc., are obtained.

«ALUMINUM ALLOYS.»

M. H. Pecheux has contributed to the _Comptes Rendus_, from time to
time, the results of his investigations into the alloys of aluminum
with soft metals, and the following constitutes a brief summary of his
observations:

«Lead.»—When aluminum is melted and lead is added in proportion
greater than 10 per cent, the metals separate on cooling into three
layers—lead, aluminum, and between them an alloy containing from 90 to
97 per cent of aluminum. {49} The alloys with 93, 95, and 98 per cent
have densities of 2.745, 2.674, and 2.600 respectively, and melting
points near that of aluminum. Their color is like that of aluminum,
but they are less lustrous. All are malleable, easily cut, softer
than aluminum, and have a granular fracture. On remelting they become
somewhat richer in lead, through a tendency to liquation. They do not
oxidize in moist air, nor at their melting points. They are attacked in
the cold by hydrochloric and by strong sulphuric acid, with evolution
of hydrogen, and by strong nitric acid when hot; strong solution of
potassium hydroxide also attacks them. They are without action on
distilled water, whether cold or hot.

«Zinc.»—Well-defined alloys were obtained, corresponding to the
formulas Zn_〈3〉Al, Zn_〈2〉Al, ZnAl, ZnAl_〈2〉, ZnAl_〈3〉, ZnAl_〈4〉,
ZnAl_〈6〉, ZnAl_〈10〉, ZnAl_〈12〉. Their melting points and densities
all lie between those of zinc and aluminum, and those containing most
zinc are the hardest. They are all dissolved by cold hydrochloric acid
and by hot dilute nitric acid. Cold concentrated nitric acid attacks
the first three, and cold dilute acid the first five. The Zn_〈3〉Al,
ZnAl_〈6〉, ZnAl_〈10〉, and ZnAl_〈12〉 are only slightly affected by
cold potassium-hydroxide solution; the others are strongly attacked,
potassium zincate and aluminate probably being formed.

«Tin.»—A filed rod of tin-aluminum alloy plunged in cold water gives
off for some minutes bubbles of gas, composed of hydrogen and oxygen
in explosive proportions. An unfiled rod, or a filed rod of either
aluminum or tin, is without action, though the unfiled rod of alloy
will act on boiling water. The filed rod of alloy, in faintly acid
solution of copper or zinc sulphate, becomes covered with a deposit
of copper or zinc, while bubbles of oxygen are given off. M. Pecheux
believes that the metals are truly alloyed only at the surface, and
that filing lays bare an almost infinitely numerous series of junctions
of the two metals, which, heated by the filing, act as thermocouples.

«Bismuth.»—By the method used for lead, bismuth alloys were obtained
containing 75, 85, 88, and 94 per cent of aluminum, with densities
2.86, 2.79, 2.78, and 2.74 respectively. They were sonorous, brittle,
finely grained, and homogeneous, silver-white, and with melting points
between those of their constituents, but nearer that of aluminum. They
are not oxidized in air at the temperature of casting, but are readily
attacked by acids, concentrated or dilute, and by potassium-hydroxide
solution. The filed alloys behave like those of tin, but still more
markedly.

«Magnesium.»—These were obtained with 66, 68, 73, 77, and 85 per cent
of aluminum, and densities 2.24, 2.47, 2.32, 2.37, 2.47. They are
brittle, with large granular fracture, silver-white, file well, take
a good polish, and have melting points near that of aluminum. Being
viscous when melted, they are difficult to cast, and when slowly cooled
form a gray, spongy mass which cannot be remelted. They do not oxidize
in air at the ordinary temperatures, but burn readily at a bright-red
heat. They are attacked violently by acids and by potassium-hydroxide
solution, decompose hydrogen peroxide, and slowly decompose water even
in the cold.

«Tin, Bismuth, and Magnesium.»—The action of water on these alloys
just referred to has been recently demonstrated on a larger scale, 5
to 6 cubic centimeters of hydrogen having been obtained in 20 minutes
from 2 cubic centimeters of the filed tin alloy. The bismuth alloy
yielded more hydrogen than the tin alloy, and the magnesium alloy more
than the bismuth alloy. The oxygen of the decomposed water unites
with the aluminum. Larger quantities of hydrogen are obtained from
copper-sulphate solution, apart from the decomposition of this solution
by precipitation of copper at the expense of the metal alloyed with the
aluminum. The alloys of aluminum with zinc and lead do not decompose
pure water, but do decompose the water of copper-sulphate solution,
and, more slowly, that of zinc-sulphate solution.

Aluminum is a metal whose properties are very materially influenced
by a proportionately small addition of copper. Alloys of 99 per cent
aluminum and 1 per cent of copper are hard, brittle, and bluish in
color; 95 per cent of aluminum and 5 per cent of copper give an alloy
which can be hammered, but with 10 percent of copper the metal can no
longer be worked. With 80 per cent and upward of copper are obtained
alloys of a beautiful yellow color, and these mixtures, containing
from 5 to 10 percent of aluminum and from 90 to 95 per cent of copper,
are the genuine aluminum bronzes. The 10-per-cent alloys are of a pure
golden-yellow color; with 5 per cent of aluminum they are reddish
yellow, like gold heavily alloyed with copper, and a 2-per-cent
admixture is of an almost pure copper red. {50} As the proportion of
copper increases, the brittleness is diminished, and alloys containing
10 per cent and less of aluminum can be used for industrial purposes,
the best consisting of 90 per cent of copper and 10 of aluminum. The
hardness of this alloy approaches that of the general bronzes, whence
its name. It can be stretched out into thin sheets between rollers,
worked under the hammer, and shaped as desired by beating or pressure,
in powerful stamping presses. On account of its hardness it takes a
fine polish, and its peculiar greenish-gold color resembles that of
gold alloyed with copper and silver together.

Alloys with a still greater proportion of copper approach this metal
more and more nearly in their character; the color of an alloy, for
instance, composed of 95 per cent of copper and 5 per cent of aluminum,
can be distinguished from pure gold only by direct comparison, and the
metal is very hard, and also very malleable.

«Electrical Conductivity of Aluminum Alloys.»—During three years’
exposure to the atmosphere, copper-aluminum alloys in one test
gradually diminished in conductivity in proportion to the amount of
copper they contained. The nickel-copper aluminum alloys, which show
such remarkably increased tensile strength as compared with good
commercial aluminum, considerably diminished in total conductivity.
On the other hand, the manganese-copper aluminum alloys suffered
comparatively little diminution in total conductivity, and one of them
retained comparatively high tensile strength. It was thought that an
examination of the structure of these alloys by aid of microphotography
might throw some light on the great difference which exists between
some of their physical properties. For instance, a nickel-copper
aluminum alloy has 1.6 times the tensile strength of ordinary
commercial aluminum. Under a magnification of 800 diameters practically
no structure could be discovered. Considering the remarkable
crystalline structure exhibited by ordinary commercial aluminum near
the surface of an ingot, when allowed to solidify at an ordinary rate,
the want of structure in these alloys must be attributed to the process
of drawing down. The inference is that the great difference which
exists between their tensile strengths and other qualities is not due
to variation in structure.

«Colored Alloys of Aluminum.»—A purple scintillating composition is
produced by an alloyage of 78 parts of gold and 22 parts aluminum.
With platinum a gold-colored alloy is obtained; with palladium a
copper-colored one; and with cobalt and nickel one of a yellow color.
Easily fusible metals of the color of aluminum give white alloys. Metal
difficult of fusion, such as iridium, osmium, titanium, etc., appear in
abnormal tones of color through such alloyages.

«Aluminum-Brass.»—Aluminum, 1 per cent; specific gravity, 8.35; tensile
strength, 40. Aluminum, 3 per cent; specific gravity, 8.33; tensile
strength, 65. The last named is harder than the first.

«Aluminum-Copper.»—Minikin is principally aluminum with a small
percentage of copper and nickel. It is alloyed by mixing the aluminum
and copper, then adding the nickel. It resembles palladium and is very
strong.

«Aluminum-Silver.»—I.—Silver, 3 per cent; aluminum, 97 per cent. A
handsome color.

II.—A silver aluminum that is easily worked into various articles
contains about one-fourth silver and three-fourths of aluminum.

«Aluminum-Tin.»—Bourbon metal is composed of equal parts of aluminum
and tin; it solders readily.

«Aluminum-Tungsten.»—A new metal alloy consisting of aluminum and
tungsten is used of late in France in the construction of conveyances,
especially carriages, bicycles, and motor vehicles. The French call
it partinium; the composition of the new alloy varies according to
the purposes for which it is used. It is considerably cheaper than
aluminum, almost as light, and has a greater resistance. The strength
is stated at 32 to 37 kilograms per square millimeter.

«Aluminum-Zinc.»—Zinc, 3 per cent; aluminum, 97 per cent. Very ductile,
white, and harder than aluminum.

AMALGAMS: See Fusible Alloys.

«Anti-Friction Bearing or Babbitt Metals.»—These alloys are usually
supported by bearings of brass, into which it is poured after they have
been tinned, and heated and put together with an exact model of the
axle, or other working piece, plastic clay being previously applied,
in the usual manner, as a lute or outer mold. Soft gun metal is also
excellent, and is much used for bearings. They all become less heated
in working than the {51} harder metals, and less grease or oil is
consequently required when they are used.

I.—An anti-friction metal of excellent quality and one that has been
used with success is made as follows: 17 parts zinc; 1 part copper;
1 1⁠/⁠2 parts antimony; prepared in the following way: Melt the copper
in a small crucible, then add the antimony, and lastly the zinc, care
being taken not to burn the zinc. Burning can be prevented by allowing
the copper and antimony to cool slightly before adding the zinc. This
metal is preferably cast into the shape desired and is not used
as a lining metal because it requires too great a heat to pour. It
machines nicely and takes a fine polish on bearing surfaces. It has the
appearance of aluminum when finished. Use a lubricating oil made from
any good grade of machine oil to which 3 parts of kerosene have been
added.

II.—Copper, 6 parts; tin, 12 parts; lead, 150 parts; antimony, 30
parts; wrought iron, 1 part; cast iron, 1 part. For certain purposes
the composition is modified as follows: Copper, 16 parts; tin, 40
parts; lead, 120 parts; antimony, 24 parts; wrought iron, 1 part; cast
iron, 1 part. In both cases the wrought iron is cut up in small pieces,
and in this state it will melt readily in fused copper and cast iron.
After the mixture has been well stirred, the tin, lead, and antimony
are added; these are previously melted in separate crucibles, and when
mingled the whole mass is again stirred thoroughly. The product may
then be run into ingots, to be employed when needed. When run into the
molds the surface should be well skimmed, for in this state it oxidizes
rapidly. The proportions may be varied without materially affecting the
results.

III.—From tin, 16 to 20 parts; antimony, 2 parts; lead, 1 part; fused
together, and then blended with copper, 80 parts. Used where there is
much friction or high velocity.

IV.—Zinc, 6 parts; tin, 1 part; copper, 20 parts. Used when the metal
is exposed to violent shocks.

V.—Lead, 1 part; tin, 2 parts; zinc, 4 parts; copper, 68 parts. Used
when the metal is exposed to heat.

VI.—Tin, 48 to 50 parts; antimony, 5 parts; copper, 1 part.

VII.—(Fenton’s.) Tin, with some zinc, and a little copper.

VIII.—(Ordinary.) Tin, or hard pewter, with or without a small portion
of antimony or copper. Without the last it is apt to spread out under
the weight of heavy machinery. Used for the bearings of locomotives,
etc.

The following two compositions are for motor and dynamo shafts: 100
pounds tin; 10 pounds copper; 10 pounds antimony.

83 1⁠/⁠2 pounds tin; 8 1⁠/⁠4 pounds antimony; 8 1⁠/⁠4 pounds copper.

IX.—Lead, 75 parts; antimony, 23 parts; tin, 2 parts.

X.—Magnolia Metal.—This is composed of 40 parts of lead, 7 1⁠/⁠2 parts
of antimony, 2 1⁠/⁠2 of tin, 1⁠/⁠8 of bismuth, 1⁠/⁠8 of aluminum, and
1⁠/⁠4 of graphite. It is used as an anti-friction metal, and takes its
name from its manufacturer’s mark, a magnolia flower.

ARGENTAN: See German Silver, under this title.

«BELL METAL.»

The composition of bell metal varies considerably, as may be seen below:

I.—(Standard.) Copper, 78 parts; tin, 22 parts; fused together and
cast. The most sonorous of all the alloys of copper and tin. It is
easily fusible, and has a fine compact grain, and a vitreous conchoidal
and yellowish-red fracture. According to Klaproth, the finest-toned
Indian gongs have this composition.

II.—(Founder’s Standard.) Copper, 77 parts; tin, 21 parts; antimony, 2
parts. Slightly paler and inferior to No. I.

III.—Copper, 80 parts; tin, 20 parts. Very deep-toned and sonorous.
Used in China and India for the larger gongs, tam-tams, etc.

IV.—Copper, 78 to 80 parts; tin, 22 to 20 parts. Usual composition of
Chinese cymbals, tam-tams, etc.

V.—Copper, 75 (= 3) parts; tin, 25 (= 1) part. Somewhat brittle. In
fracture, semivitreous and bluish-red. Used for church and other large
bells.

VI.—Copper, 80 parts; tin, 10 1⁠/⁠4 parts; zinc, 5 1⁠/⁠2 parts; lead,
4 1⁠/⁠4 parts. English bell metal, according to Thomson. Inferior to
the last; the lead being apt to form isolated drops, to the injury of
the uniformity of the alloy.

VII.—Copper, 68 parts; tin, 32 parts. Brittle; fracture conchoidal
and ash-gray. Best proportions for house bells, hand bells, etc.; for
which, however, 2 of copper and 1 of tin is commonly substituted by the
founders.

VIII.—Copper, 72 parts; tin, 26 1⁠/⁠2 parts; iron, 1 1⁠/⁠2 parts. Used
by the Paris houses for the bells of small clocks.

IX.—Copper, 72 parts; tin, 26 parts; zinc, 2 parts. Used, like the
last, for very small bells.

X.—Copper, 70 parts; tin, 26 parts; {52} zinc, 2 parts. Used for the
bells of repeating watches.

XI.—Melt together copper, 100 parts; tin, 25 parts. After being cast
into the required object, it should be made red-hot, and then plunged
immediately into cold water in order to impart to it the requisite
degree of sonorousness. For cymbals and gongs.

XII…

source: Project Gutenberglicence: Public domain (per item)year: —id: 53143citation: https://www.gutenberg.org/ebooks/53143characters: 200,001

record · JSON · record JSON

Related services and records

Services

  • Estate — measured countries, lanes and facts
  • Intel — live corroborated events
  • Legal — statutes, cases and citations
  • Encyclopedia — articles with inline sources
  • Space — launches, satellites and orbits
  • Search — federated search and reports
  • Pass — passport account and SSO
  • Corpora — read-only corpus origins
  • e01 — self-hosted corpora and tools

Text and metadata only; each target carries its own sources. Missing data is published as no-data, never estimated.