gutenberg.go-v.org

Photo-engraving, Photo-etching and Photo-lithography in Line and Half-tone

The Project Gutenberg eBook of Photo-engraving, Photo-etching and Photo-lithography in Line and Half-tone This eBook is for the use of anyone anywhere in the United States and most other parts of the world at no cost and with almost no restrictions whatsoever. You may copy it, give it away or re-use it under the terms of the Project Gutenberg License included with this eBook or online at www.gutenberg.org. If you are not located in the United States, you will have to check the laws of the country where you are located before using this eBook. Title: Photo-engraving, Photo-etching and Photo-lithography in Line and Half-tone Author: W. T. Wilkinson Editor: Edward L. Wilson Release date: June 19, 2016 [eBook #52378] Most recently updated: October 23, 2024 Language: English Other information and formats: www.gutenberg.org/ebooks/52378 Credits: Produced by Chris Curnow, RichardW, and the Online Distributed Proofreading Team at http://www.pgdp.net (This file was produced from images generously made available by The Internet Archive) *** START OF THE PROJECT GUTENBERG EBOOK PHOTO-ENGRAVING, PHOTO-ETCHING AND PHOTO-LITHOGRAPHY IN LINE AND HALF-TONE *** Photo-engraving, Photo-etching, and Photo-lithography in Line and Half-tone; Also Collotype and Heliotype; By W. T. Wilkinson, Revised and Enlarged by Edward L. Wilson. [Illustration: John C. Moss, Prest. R. B. Moss, Supt. M. A. Moss, Treasurer. J. E. Ramsey, Secretary. H. A. Jackson, Asst. Secy. Moss Engraving Co. 535 Pearl St., New York Illustrations of every De

source: Project Gutenberglicence: Public domain (per item)database: /home/dbs/gutenberg.dbmode: tablerecords: 544887 (max_rowid)citation: https://www.gutenberg.org/

The Project Gutenberg eBook of Photo-engraving, Photo-etching and Photo-lithography in Line and Half-tone

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: Photo-engraving, Photo-etching and Photo-lithography in Line and Half-tone

Author: W. T. Wilkinson

Editor: Edward L. Wilson

Release date: June 19, 2016 [eBook #52378]
Most recently updated: October 23, 2024

Language: English

Other information and formats: www.gutenberg.org/ebooks/52378

Credits: Produced by Chris Curnow, RichardW, and the Online
Distributed Proofreading Team at http://www.pgdp.net (This
file was produced from images generously made available
by The Internet Archive)

*** START OF THE PROJECT GUTENBERG EBOOK PHOTO-ENGRAVING, PHOTO-ETCHING AND PHOTO-LITHOGRAPHY IN LINE AND HALF-TONE ***

Photo-engraving, Photo-etching, and Photo-lithography in Line and
Half-tone; Also Collotype and Heliotype; By W. T. Wilkinson, Revised
and Enlarged by Edward L. Wilson.

[Illustration: John C. Moss, Prest. R. B. Moss, Supt. M. A. Moss,
Treasurer. J. E. Ramsey, Secretary. H. A. Jackson, Asst. Secy.

Moss Engraving Co. 535 Pearl St., New York

Illustrations of every Description, FOR BOOKS, NEWSPAPERS, CIRCULARS,
&c., &c.

Send green stamp for circular. Send photograph, drawing or print, for
estimate.

our Specialty. Fine Illustrated Circulars by our Moss-Type Process.]

[Illustration: SPECIMEN OF “MOSS-TYPE” ENGRAVED BY THE MOSS ENGRAVING
CO., 535 PEARL STREET, NEW YORK.]

[Illustration: SPECIMEN OF “MOSS-TYPE” ENGRAVED BY THE MOSS ENGRAVING
CO., 535 PEARL STREET, NEW YORK.]

[Illustration: SPECIMEN OF “MOSS-TYPE” ENGRAVED BY THE MOSS ENGRAVING
CO., 535 PEARL STREET, NEW YORK.]

[Illustration: G. CRAMER, ST. LOUIS.

HALF-TONE ZINC ETCHING. (MOSSTYPE.) FROM A PHOTOGRAPH.]

PHOTO-ENGRAVING, PHOTO-ETCHING,

AND

PHOTO-LITHOGRAPHY

IN LINE AND HALF-TONE;

ALSO,

COLLOTYPE AND HELIOTYPE.

BY

W. T. WILKINSON,
OF LONDON.

REVISED AND ENLARGED BY

EDWARD L. WILSON,

EDITOR OF “THE PHILADELPHIA PHOTOGRAPHER,” AUTHOR OF “WILSON’S
PHOTOGRAPHICS,” “WILSON’S QUARTER CENTURY IN PHOTOGRAPHY,”
“PHOTOGRAPHIC MOSAICS,” ETC.

AMERICAN (THIRD) EDITION.

[Illustration]

_The camera is mightier than the pen or the pencil._

NEW YORK:
PUBLISHED BY EDWARD L. WILSON,
NO. 853 BROADWAY.
1888.

Entered according to Act of Congress in the year 1888, by

EDWARD L. WILSON,

In the office of the Librarian of Congress, at Washington, D. C.

[Illustration]

PREFACE.

The many kind letters I have received from America with regard to
what must be called my first crude effort at bookmaking, prompted the
idea—after issuing a second and revised edition in England—of making an
attempt to cater for the inhabitants of Greater Britain, which, under
the able editorship of MR. EDWARD L. WILSON will, I have no doubt, meet
with approbation and be useful. I have made many important additions to
the last English edition.

W. T. WILKINSON.

LEICESTER, ENGLAND.

* * * * *

Besides revising the English edition and incorporating in proper place
such additions as I have found useful in practice, I have boiled down
the best points from current publications in France and Germany, and
added them.

More still, with high regard for the author, I add chapters and parts
from, the _Handbuch der Chemigraphie und Photochemigraphie_, by Mr. J.
O. Mörch. Thus, I believe, this work is made complete to date. All the
rest must come to the worker, from industrious, careful practice.

Very rapid progress has been made in photo-reproductive processes
during the past two years, and improvements are announced almost
weekly. I invite all interested to keep me informed of what they
discover. If I am supplied with the proper addresses I shall publish
and distribute what I learn.

EDWARD L. WILSON.

NEW YORK, May, 1888.

LIST OF ILLUSTRATIONS.

The Reversing Mirror . . . 10

The Dark-room . . . 25

The Plate-support . . . 37

The Whirler . . . 42

The Copying Camera . . . 67

Example of Zinc Etching (low) . . . 88

Example of Zinc Etching (high) . . . 90

Example of Zinc Etching (round) . . . 92

The Caliber-bridge . . . 93

The Sieve . . . 98

The Heating Lamp . . . 98

The Washing Table . . . 98

Example of Photo-engraving . . . 117

Example of Half-tone Engraving . . . 118

The Dusting-box . . . 124

The Transfer-board . . . 141

The Drying-oven . . . 167

Support for the Drying-oven . . . 168

Jacket for the Drying-oven . . . 168

Copper Tank for the Drying-oven . . . 168

Interior plan for the Drying-oven . . . 169

A New Drying-oven . . . 174

The Universal Copying Machine . . . 178

CONTENTS.

PART I. PHOTO-ENGRAVING IN LINE.

CHAPTER I.
APPLIANCES FOR MAKING PHOTOGRAPHIC NEGATIVES . . . 9

CHAPTER II.
THE WET COLLODION PROCESS . . . 11

CHAPTER III.
PHOTOGRAPHIC MANIPULATIONS . . . 24

CHAPTER IV.
APPARATUS FOR PRINTING UPON ZINC . . . 39

CHAPTER V.
PRINTING ON ZINC IN ALBUMEN . . . 45

CHAPTER VI.
PRINTING ON ZINC IN BITUMEN . . . 48

CHAPTER VII.
DIRECT TRANSFERS TO ZINC . . . 51

CHAPTER VIII.
ETCHING LINE TRANSFERS . . . 55

PART II. PHOTO-ENGRAVING IN HALF-TONE.

CHAPTER I.
RETROSPECTIVE . . . 63

CHAPTER II.
MAKING GRAINED NEGATIVES . . . 65

CHAPTER III.
ETCHING IN HALF-TONE . . . 69

CHAPTER IV.
PRINTING FROM THE BLOCK . . . 72

CHAPTER V.
THE TRANSFER OF THE DRAWING, AND ITS TREATMENT
BEFORE ETCHING . . . 73

CHAPTER VI.
HINTS FROM ALL SOURCES . . . 94

PART III. PHOTO-ENGRAVING ON COPPER.

CHAPTER I.
SUBJECTS IN LINE . . . 119

CHAPTER II.
HALF-TONE INTAGLIOS . . . 122

CHAPTER III.
HALF-TONE INTAGLIOS—(_Continued_) . . . 124

CHAPTER IV.
HALF-TONE INTAGLIOS. ELECTROTYPING METHODS . . . 127

PART IV. PHOTO-LITHOGRAPHY IN LINE.

CHAPTER I.
PHOTO-LITHOGRAPHY IN LINE . . . 129

CHAPTER II.
PAPER TRANSFERS . . . 132

CHAPTER III.
PAPER TRANSFERS—(_Continued_) . . . 136

CHAPTER IV.
TOOVEY’S NEGATIVE TRANSFER PROCESS . . . 139

CHAPTER V.
PHOTO-LITHO. TRANSFERS . . . 140

PART V. PHOTO-LITHOGRAPHY IN HALF-TONE.

CHAPTER I.
PHOTO-LITHOGRAPHY IN HALF-TONE . . . 143

CHAPTER II.
INK PHOTOS . . . 144

CHAPTER III.
HUSBAND’S PAPYROTINT PROCESS . . . 147

PART VI. COLLOGRAPHIC PRINTING.

CHAPTER I.
HALF-TONE PHOTOGRAPHIC NEGATIVES . . . 151

CHAPTER II.
THE HELIOTYPE PROCESS . . . 152

CHAPTER III.
THE COLLOTYPE PROCESS . . . 163

CHAPTER IV.
PRINTING FROM THE COLLOTYPE PLATE . . . 171

CHAPTER V.
THE NEW HOME PRINTING PROCESS . . . 178

|xv|

INTRODUCTION.

The improvements made within the last twenty years in the art of
printing books have not, until recently, been kept pace with by the
methods of illustration. Wood engraving, except for high class and
expensive editions, was crude, whilst the use of engravings from copper
or steel, or of lithographs, was also restricted to short and expensive
editions.

The introduction of the zinc-etching process, in which the picture is
first drawn in line, or stipple, or chalk, upon lithographic transfer
paper, then transferred to a plate of zinc and subjected to a process
of etching in various baths of acid water, marks a new era, replete
with great improvements in cheapness, facility of production, and
artistic results.

This new process had scarcely been in good working order before it was
seen that great improvements might be made by enlisting photography in
its service; because in its original form it was necessary that the
design be made of the same size as the finished block, which, in many
cases, added too much to the expense. But by introducing photography,
the size of the original was of no moment; the lens could easily reduce
that, and at the same time preserve the proportions, as well as fine
down any crudity in the drawing.

The first methods of producing a photo-transfer, were by making
a negative from the original, then paper coated with bichromated
gelatine was exposed under this negative, and the sensitive gelatine,
corresponding with the transparent portions of the negative
(representing the lines of the original), being exposed to the action
of light was made non-absorbent of water, whilst the sensitive gelatine
representing the white portion of the original being protected from the
action of light by the dark portion of the negative, still retained its
affinity for water. The consequence was that when a roller charged with
fatty ink was applied to the wet print, the exposed portions of the
gelatine took the ink, but the white portion being charged with water
rejected it, the result being a replica of the original in a fatty
ink. This was used as an ordinary lithographic transfer and could be
transferred to zinc and etched in relief. |xvi|

Such a process was not perfect, and was not suitable for subjects which
necessarily should be to scale. So the next improvement was to place
a plain mirror between the lens and sensitive plate, so producing a
negative in its proper position as regards right and left; then from
this reversed negative a print in fatty ink could be made direct on the
zinc.

These transfers on paper, or direct prints on the zinc, are restricted
entirely to what are generally termed “subjects in line,” such as
architectural drawings, plans, woodcuts, engravings from steel or
copper plates, or lithographs in pure line, in chalk, or in stipple.
The attainment of effect of half tones by graduated works of color,
thinner or thicker, or the smooth, delicate gradations of a photograph,
are not permissible in relief blocks of this kind, although for
short numbers this class of subject could be utilized by employing
the collotype, heliotype, or lichtdruck methods, which render the
half-tones without (visible) breaking up of the gradations.

The next step was to perfect the various (published first in 1854 by
Fox Talbot) methods of mechanically breaking up the half-tones of a
photograph, and so giving a means whereby a photograph in all its
delicacy may be used to illustrate a letter-press article.

Of course, during the progress of rendering photography applicable for
relief blocks, its usefulness for intaglio printing was not neglected.
And now having entered into very close competition with wood engraving
and by modification of the collotype methods, with lithography,
photography can now be used for the production of intaglio plates, in
half-tones as well as in line.

The methods by which the above results are attained furnish the text
of the pages to follow; and as each and every method given has been
tried by the author, the reader may be satisfied that the manual is, as
claimed, _practical_.

W. T. WILKINSON.

|9|

PHOTO-ENGRAVING, ETCHING, AND LITHOGRAPHY.

PART I.

PHOTO-ENGRAVING IN LINE.

CHAPTER I.

APPLIANCES FOR MAKING PHOTOGRAPHIC NEGATIVES.

For all methods of heliographic printing a suitable photographic
negative is absolutely necessary, and to produce that negative good
apparatus and pure chemicals, used with skill and intelligence, are
indispensable.

The studio must be well lighted, with a perfectly firm floor. The
dark-room should be kept for negative work only (the room where the
zinc printing is carried on being a separate room). There must be a
roomy sink in front of a good-sized window covered with a non-actinic
medium (yellow, not orange), such as two thicknesses of golden fabric,
so as to have plenty of light to see the progress of development by.

The copying camera must have a long bellows and should not be less
than 12 by 10, fitted with rack-work, so as to be able to get absolute
sharpness in focussing.

It will be a great advantage, and aid in adjusting the position on the
focussing screen of the drawings to be copied, if a vertical line be
drawn, and another horizontally, so that they bisect each other exactly
in the centre; then _from the centre_, mark and number each inch and
half inch upon each of the four arms of the cross; it can then be seen
at a glance not only that the picture is in the centre, but also that
it is about the right size. |10|

The dark slide must be light-tight, and made strong rather than for
portability.

The lens should be rectilinear, and should be capable of covering the
largest size plate the camera will take quite sharp to the corners. For
a 12 by 10 plate a lens with an equivalent focus of about 18 inches
will be best.

[Illustration: Fig. 1.]

To the lens must be fitted a reversing mirror of silvered glass,
mounted behind the lens by preference, as such a style of mounting
not only protects the surface of the mirror from the air, but keeps
extraneous light from affecting the brilliancy of the image. (Fig. 1.)

The camera must be mounted upon a solid table fixed upon small grooved
or flanged wheels, such wheels running either upon rails fixed upon
or in grooves cut into the floor, at right angles to the wall against
which the copying board is fitted.

The copying easel is placed perpendicularly in front of, and perfectly
parallel with, the camera. As a mirror is used, the camera is sideways
to the object, not facing it, as in copying direct.

The easel should be so contrived that it can be raised or lowered, and
moved right and left, which double motion is managed by having the
easel double; the up and down motion should be obtained by hanging
the back portion like a window sash, the weights being exactly the
weight of the whole easel, and the pulleys over which the cords go, not
running too freely.

At the top and bottom of the back portions of the easel are projecting
strips with a rabbet deep enough to allow the front or copying board to
slide sideways, but not loosely; this front board should be painted a
dead black with white lines in the centre from top to bottom and from
side to side, said lines being divided into inches and half inches,
from the centre, so that the drawing may be pinned in the exact centre
without trouble.

A convenient size for a copying board is 4 feet high by 5 feet wide.

In connection with the camera, the only thing left to describe is the
focussing cloth, which should be quite opaque, and of ample size to
exclude all extraneous light from behind when focussing.

For focussing the image absolutely sharp, a magnifying glass may be
required.

|11|

CHAPTER II.

THE WET COLLODION PROCESS.

THE COLLODION.

Alcohol 30 ounces.
Ether 40 ounces.
Schering’s Celloidin* 1-1/2 cakes.

* Hance’s D. C. gun-cotton may be used instead of the
celloidin.

Cut the celloidin into thin strips, or, if it be hard, break it up in a
clean mortar, and dissolve in the above mixture of alcohol and ether.
When dissolved, this forms the collodion.

THE IODIZER

is composed of:

Bromide of Zinc 150 grains.
Iodide of Zinc 350 grains.
Alcohol 10 ounces.

When the salts are dissolved, filter and add to the collodion.

The filtering is best done by placing a pledget of cotton-wool in the
neck of a glass funnel and passing the iodizer through it. To prevent
evaporation, lay a glass plate over the funnel.

The iodizer being added to the collodion, shake them up thoroughly
and allow to stand for a week to settle, then decant into convenient
bottles; this collodion is ready for use in a week, but will improve
with age up to six months, after which time it should be mixed with new.

When coating plates with collodion, it is not a wise plan to pour the
surplus from the plate back into the bottle from which it was poured.
Pour it into another, kept handy for the purpose, the contents of
which, at the end of the day’s work, empty into the stock bottle after
such a quantity as is sufficient for next day’s consumption has been
decanted into the pourer.

The best bottle from which to pour the collodion upon the plate is the
tall capped bottle sold by the dealers as collodion pourers. |12|

THE NITRATE OF SILVER BATH (1).

The silver bath is a most important factor in the production of good
negatives. It must be compounded with care and used with skill.

To make it, dissolve 6 ounces of nitrate of silver in 10 ounces of
water, then add 10 drops of collodion, and shake up well; then add 70
ounces of water, and let it stand all night; then filter through a
pledget of cotton-wool packed loosely in the neck of a glass funnel,
into a clean bottle or jug; then add 1 drachm of nitric acid and let
stand all night before trying. Such bottle or jug, and also the glass
funnel, must be kept solely for use with the silver bath.

The bath holder may be an upright vessel of the ordinary pattern,
with a dipper with which to lower the plate into the solution; or it
may be a flat dish with a cover to keep out light and dust, using a
silver hook to lift the plate from the solution; if the former shape be
chosen, let the dipper be of glass, porcelain, silver wire, or of wood
soaked in melted paraffine, but on no account of ebonite, as such a
dipper will cause spots, and derange the bath sooner or later.

If a flat dish be used, the best form is of wood lined with asphaltum,
hanging on a cradle, the lower end being a well to hold the solution;
in this form of bath the plate, after sensitizing, is drained
thoroughly before taking it out. This is a great convenience, as not
only is silver solution saved, but the dark slide will last much longer.

The bath solution made up as above will be the right strength for
work, but as every plate sensitized therein, takes away its modicum
of silver, after a certain time it must be strengthened, as it is
essential for the production of good work that the solution be kept at
a proper strength. The best way of doing this is to add a drachm or two
of saturated solution of nitrate of silver, after each day’s work has
been done, and if the solution be worked in a flat bath, it will be as
well to pour it into a jug and filter it before using again; with an
upright holder, this filtering will only require to be done about once
or twice a week, as any particles of dust, etc., subside and have not
the same chance of falling upon the film as in a flat bath; but the
addition of the silver solution should be made, and the solution well
stirred up with the dipper.

In course of time a silver bath will become contaminated with organic
matter from various causes, and can also be supersaturated with ether
and alcohol—with iodo-bromo or nitrate of zinc, and will either refuse
to work, or only |13| yield imperfect films and thin images. In such
cases the best plan will be to take 20 ounces of the solution, dilute
it with clean water 60 ounces, filter, and add 6 ounces of nitrate of
silver, and again filter, when a new bath will be the result.

The silver in the rejected portion of the old bath should be
precipitated as a chloride, by the addition of a solution of common
salt, the precipitate dried and sent to a refiner, together with the
ashes of the filtering papers and blotting-paper used to drain the
plates upon, or to wipe the backs of the plates after leaving the bath
and before putting them into the dark slide.

The silver solution named above, is suitable for negatives of subjects
in line, but for the production of negatives with delicate half
tones, such as portraits, landscapes, or of the many subjects which
are photographed direct, then it will be necessary to provide another
bath solution, made and managed in the same way, but only containing
sufficient nitric acid to just redden litmus paper, as a bath gives the
finest half-tones when nearly neutral, or only slightly acid. It should
be remembered that the deepest shadows are represented by clear glass
in the negative, to insure which would be impossible with the silver
solution inclining ever so slightly toward alkalinity.

The nitrate of silver bath may be made up with distilled water, if
pure—that is, if the water is bona fide distilled and not merely from
waste steam; if this cannot be guaranteed, the best plan will be to get
a gallon of tap water, dissolve in it one ounce of nitrate of silver,
then add saturated solution of bicarbonate of soda, until an alkaline
reaction to litmus paper takes place, then place the lot in white glass
bottles, and expose to the action of light for three or four days.
During that time the solution will, first of all, turn black, and
then will gradually become quite clear, the organic matter—which if
not removed, would have caused trouble—falling in a black mass to the
bottom.

Now filter the purified water and use it for compounding the nitrate of
silver bath, but do not use it for any other purpose.

The strength of a nitrate of silver bath, for line work, should be
thirty grains of nitrate of silver to each ounce of water, and should
not be allowed to fall below twenty-five; and for half-tone negatives,
nitrate of silver should be thirty-five, and not lower than thirty
grains to the ounce.

Be sure to keep all funnels, bottles, and dishes used for the silver
bath, separate and distinct from all others, and never use them for any
other purpose. |14|

THE NITRATE OF SILVER BATH (2).

In the ancient days of photography, when, to say it was possible to
prepare a dry plate nearly as sensitive as a wet collodion plate, was
to excite the risible faculties of the audience, the above heading
might almost always be seen in the journals, and the amount of matter
written under that heading would fill many good-sized volumes. Some
writers went into the subject in a very elaborate manner, whilst others
would counsel very simple methods of preparation and management.

The directions given above for making a bath solution for line
negatives, will, if carried out carefully and cleanly, at once yield a
solution giving good negatives. After the bath has been mixed, either
with distilled water, ordinary tap water (_in iron districts tap water
should not be used_), or water that has been sunned and filtered, as
soon as the bulk has been made up to the eighty ounces, the solution
should be put away all night before it is tried, then in the morning
filter it carefully through a pledget of cotton-wool stuffed loosely in
the neck of a perfectly clean funnel, into a perfectly clean bottle or
jug, which must be kept entirely for use of the silver solution. When
the bath solution has been filtered it should be _perfectly clear_; if
it is at all cloudy or turbid, the filtration must be repeated.

When the solution is perfectly clear and bright, pour sufficient into
a perfectly clean porcelain, glass, or papier-maché dish, then take
a clean plate (polished, or albumenized) and coat it with collodion;
close the door of the dark-room, and when the film of collodion
is perfectly set, raise one end of the dish containing the silver
solution, place one edge of the collodionized plate against the bottom
of the upper edge of the dish, then drop the plate upon the bottom
of the dish, and at the same time lower the dish; by this means the
silver solution will flow in an even wave over the surface of the
collodionized plate; now place the cover on the dish so as to exclude
light and dust, and allow the plate to remain in the solution for five
minutes, then with a silver hook lift the plate from the solution, and
allow it to drain (remember that no light must get into the dark-room
except what is filtered through either two thicknesses of golden
fabric, or one of canary medium); when the plate has drained so that no
solution drips from it, place it into the carrier of the dark slide;
then close the dark slide and let it remain there for five minutes,
at the end of which time remove the plate to the sink, and flood it
with sufficient developer (page 17) to just cover the film; keep this
solution flowing, to and fro, over the |15| plate for the space of
two minutes, then wash it under the tap until the surface is no longer
greasy; then apply the fixing or clearing solution (page 17) until the
whole of the yellow bromo-iodide is dissolved away; again wash, and
take the plate into the daylight.

Now comes the test; if the film is perfectly transparent, and clear as
the glass itself, the bath is all right; but if there is the slightest
deposit (which can be removed by lightly rubbing the finger along the
surface of the film), then the solution will require the addition of
a little nitric acid. After this stir it well, and after a rest of an
hour or two try again, repeat the addition of the nitric acid, and try
a plate; repeat until the film, after developing, washing, and fixing,
is perfectly clear, and free from deposit and fog.

The bath is now in proper working order, and if reinforced after
each day’s work with a sufficient quantity of saturated solution of
nitrate of silver (filtered), kept free from contamination with other
chemicals, and carefully filtered occasionally, it will remain in good
working order for at least six months, and then may be renewed by
treating as directed on page 12.

It will sometimes happen, notwithstanding that extreme care and
cleanliness is exercised in the management of the bath, that it will
not work properly, and the reason why cannot easily be discovered. In
such a case, steps must be taken to put the solution into working order.

In the case of rectifying a disordered bath, there are many methods of
procedure, but the simplest, and, as a rule, the most certain method,
is to render the solution alkaline by the addition of liquor ammonia,
adding the ammonia a little at a time; then, after well shaking, test
it with red litmus paper and continue the addition of ammonia until
the red litmus paper is turned blue. In this alkaline condition the
solution should be poured into a large flat dish, and exposed to the
action of the sun. That will speedily reduce and throw down in the form
of a black precipitate, any organic matter that may be in the bath,
and at the same time the heat of the sun will cause evaporation of the
ether and alcohol left in the solution by the collodion plates.

The bath solution should be exposed to the sun for two or three days,
or until such time as suffices to render the solution clear, and the
precipitate entirely separated out. But this cannot take place unless
the solution is decidedly alkaline, the presence of acid stopping the
action of light.

Do not be in a hurry about doctoring a bath solution (in fact, it
will be far best to have two solutions, one in use and one either
resting or being doctored), but give the light plenty of time to
reduce the organic matter, and also to |16| volatilize the ether and
alcohol; then filter the solution through filtering paper (don’t use
blotting-paper), as if it is attempted to filter through a pledget of
cotton-wool the fine precipitate of organic matter quickly clogs the
wool and stops the filtering.

The doctored solution being filtered, test it with a piece of perfectly
fresh, blue litmus paper, and add nitric acid, drop by drop—shaking
well between the additions of acid—until the blue litmus paper just
turns red. Do not add acid sufficient to make the litmus turn violently
red, unless the bath is for line negatives, as a bath for half-tone
negatives must be only just acid, whereas a bath for line work must
contain more acid.

If the color of the litmus paper shows that the alkali has been
neutralized, a plate is collodionized, then immersed in the bath for
five minutes, then drained, and placed in the dark slide, or in a dark
box for five minutes, then flooded with the iron developer (page 17);
if, upon the application of this the film should turn black, add more
nitric acid, stir up thoroughly, then try again, repeating the trials
until, upon fixing the plate with the solution of cyanide of potassium,
the film of collodion is left upon the glass plate as clear as it was
before it was immersed in the silver bath.

A little above here it is stated that less nitric acid is required in
the bath for half-tone negatives than for line work, and the question
may well be asked where may the line be drawn? The reply is that, for
half-tone work, a piece of blue litmus paper should, upon immersion
into the solution, turn red very slowly, but when the bath is required
for line negatives the blue litmus may at once indicate the presence of
acid.

After a bath solution has been renovated in the above manner, it
should be tested for strength, either by the volumetric method (by
preference), or by means of the ordinary argentometer sold by the
dealers, and, if, after testing, the strength is shown to be too
great, dilute with a sufficiency of sunned water (page 13); and if not
sufficiently strong, add crystals of nitrate of silver to make up the
strength to thirty or thirty-five grains per ounce.

A bath solution renovated as above, will generally be found to work
cleaner, and yield brighter negatives than a new solution, and it
will also, if carefully used, last longer; but it must be kept up to
a proper working strength by the occasional addition of a little of a
saturated solution of nitrate of silver.

The fact that the strength of the silver solution has got too low is
shown by the presence of semi-opaque, fantastic markings near the thick
edge of the collodion film, and also in conjunction with the presence
of organic matter in |17| the deposition under the surface of the film
of an extremely fine sand-like deposit, which, in the fixed negative,
develops into myriads of pinholes in the densest portions of the image.

THE DEVELOPING SOLUTION.

First purchase seven pounds of commercial sulphate of iron (copperas)
and put this into a gallon jug, and fill it up with boiling water
(clean); stir with a clean rod at short intervals for three or four
hours, then allow to stand until the sediment settles, and the top
portion of the solution is clear and bright; then decant as much as
possible into a bottle or bottles, and label “Saturated Solution of
Iron.” Then again fill up the jar with boiling water, stir until as
much as possible is dissolved, so as to be ready by the time the stock
in the bottle is exhausted, and repeat the process until all the
crystals are dissolved; then wash out the jar, reject the residue, and
begin again.

But bear in mind that, unless there are crystals left in the solution
after each addition of hot water, it will not be saturated; therefore,
before taking the solution into use, be sure there are undissolved
crystals in the jar.

For use, take of

Saturated Solution of Iron 10 ounces.
Acetic Acid 4 ounces.
Water 70 ounces.
Alcohol 1 ounce to 5 as required.

In the above solution, the alcohol is added to enable the developer to
readily assimilate with the sensitive film, and the quantity requisite
varies with the age of the silver bath, or, to be more correct, with
the quantity of plates sensitized therein. At first, little or no
alcohol will be required, but after a number of plates have been
sensitized the developer refuses to flow evenly, and seems disposed to
run over the edges of the plate; this is a sign that more alcohol is
required, and when more has been added the developer will flow evenly
as before; but when 80 ounces of developer require over 4 ounces of
alcohol to make it flow, it is a pretty sure sign that the bath wants
remaking.

The developer is applied to the plate after exposure, from a
straight-lipped cup, or glass measure, which should be kept for the
exclusive use of this solution, as the mixture of any of the other
solutions with it will at once counteract its working power. |18|

THE FIXING OR CLEARING SOLUTION.

Cyanide of Potassium 3 ounces.
Water 20 ounces.

This solution is highly poisonous, both in solution and vapor, so it
ought to be kept in an upright holder, the plate being lowered into
the solution on a dipper; keep the solution well covered up, so as to
prevent evaporation as much as possible.

After being in use a short time this solution will become weak and
should be strengthened by the addition in the evening of a lump or two
of cyanide and then stirred up with the dipper in the morning; the
negative must not be left in this solution too long or the density of
the film will be impaired, but must be removed and well washed directly
all the yellow iodide has been dissolved.

THE INTENSIFIER.

No. 1.

Water 80 ounces.
Chloride of Ammonium 2 ounces.

dissolve, then add:

Bichloride of Mercury 2 ounces.

dissolve, and filter.

No. 2.

Liquor Ammonia 0.880 5 ounces.
Water 20 ounces.

Solution No. 1 is best kept in an upright holder, as if kept in a flat
dish there is always the danger of cutting the skin with the glass
plate and getting the mercurial poison into the system.

No. 2 is kept in a well-stoppered bottle and only sufficient for each
plate withdrawn as required.

Another method of intensifying, for those who object to the use of
mercury, is to bleach the negative in a solution of

Ferridcyanide of Potassium (_Red Prussiate of Potash_) 6 parts.
Nitrate of Lead 4 parts.
Water 80 parts.

dissolve and filter. |19|

When the plate is bleached, wash it thoroughly under the tap, taking
care that the edges and corners of the film as well as the centre are
washed, then flood it with a sufficient quantity of

Nitric Acid 1 ounce.
Water 80 ounces.

Allow this to remain on a few seconds, then wash, and flood with a
sufficient quantity of

Sulphide of Ammonium 1 part.
Water 5 parts.

which will at once turn the film an intense black; again wash, and
flood with the nitric acid solution, and again wash; then the negative
is allowed to dry.

This method of intensifying is cheaper than the other, and if the
washes of acid between and after the other two solutions are carefully
done, and the stench of the sulphide is not objected to, then there
is little or no difference in the results; but if the acid washes
are omitted or (and) the sulphide has not been kept corked, and is
consequently not fresh, then there is great danger of a brown stain
upon the lines, which is more or less fatal to getting a good print on
zinc.

For half-tone negatives, instead of fixing or clearing with the cyanide
of potassium, the developer is washed off directly, and then they are
intensified at once by the application of a mixture of pyrogallic acid,
citric acid, and nitrate of silver, as follows:

No. 1 Solution of Pyrogallic Acid 40 grains.
Citric Acid 30 grains.
Water 20 ounces.

As much of this solution as will cover the washed plate is put into a
small cup, and flowed all over the film, then returned to the cup, and
a few drops of

Nitrate of Silver 30 grains.
Water 1 ounce.

is added. Then the mixture is poured over the film, and rocked to and
fro for a short time; the intensifier is then returned to the cup, the
negative held up to the light, and examined, and if not intense enough,
the intensifier is again applied. Great care is requisite at this
stage, as if the process be carried on too |20| far the negative will
be too intense, and will either be spoiled, or take an abnormal time
to print; practice and observation are the only guides to success. The
grand rules for half-tone negatives are, collodion free from dust, the
glass plate clean, the bath at its full strength and in good working
order, proper time allowed the plate in the sensitizing bath, well
drained, afterward a good exposure, develop until all details are out,
then wash thoroughly, intensify with judgment, wash well, fix, and
again well wash, and then, but never till then, open the dark-room door
and examine your new negative by daylight.

In making the collodion, soak the celloidin in the ether for about
twelve hours before adding the alcohol; be sure the ether is at least
0.725 specific gravity, and that the alcohol is very clean, and free
from gum. After mixing the collodion and iodizer, shake up well, but do
not do this before decanting. Always decant sufficient for next day’s
use, into the bottle used for pouring, over night, so that it gets a
chance to settle, and allows the air-bubbles to escape.

Keep the collodion in as cool a place as possible, and in decanting it
be very careful to do it away from fire, or lighted gas or paraffine,
especially where flame is below the bottle, as ether vapor does not
rise, but falls.

In hot weather and during long exposures, wet plates are very prone
to have a peculiar stain upon them, called oyster-shell markings, the
remedies for which are careful draining before putting them into the
slide, and covering the bottom of the carrier with clean filtering
paper, so that the silver solution, on draining down, is absorbed by
the bibulous paper instead of going back up the plate by capillary
attraction.

In hot weather the back of the plate, when put into the dark slide,
should be covered with a wet piece of red blotting paper, or orange
calico, _but not white_; a wet cloth laid in the camera will also tend
to keep the plate moist. These precautions, however, are not required
unless the exposure is likely to exceed a quarter of an hour.

PROTECTING THE COLLODION FILM.

A collodion film, when dry, is very delicate, and, except for line work
in the hands of an expert, will require protecting. This is usually
done by slightly warming it (when quite dry) in front of a fire, and
then pouring over a sufficient quantity of thin spirit varnish. After
the superfluous varnish is well drained off, dry by again holding it
in front of the fire. The spirit |21| varnish answers perfectly for
ordinary work, but for printing upon metal for relief blocks, or upon
glass for collotypes, it will be best to use a benzole varnish, such
as is sold by dealers for protecting the films of glass positives or
ferrotype pictures. Anthony’s “diamond” varnish is good.

But the best plan of all is to use a water varnish, made by dissolving
half an ounce of borax in a quart of boiling water, then adding a few
pieces at a time (stirring meanwhile), one pound of ordinary shellac;
if the quantity of borax named does not suffice to make all the shellac
dissolve, add more, a grain at a time, until the shellac is dissolved;
then add half an ounce of white sugar, cool and filter it.

When the negative is washed for the last time, allow it to drain, then
flood with the above solution, and let it dry. This will be found
a quicker, cleaner, and more satisfactory method of protecting the
delicate film than with the spirit varnish.

THE GLASS PLATE.

_The glass_ used as a support for the collodion film should be thin
flatted crown of the best quality, for the negatives, as a rule, are
not required again after once the zinc is etched, so that the film may
be washed off, and the glass used again, which cannot be done so often
if the glass be of bad quality; flatness is a _sine qua non_, as it has
to be subjected to heavy pressure between a zinc plate and the front
glass of a printing frame.

As a good and suitable negative is the foundation of success in
the subsequent processes, so is a properly cleaned glass plate the
foundation of a successful negative; unless the glass is chemically
clean, the collodion film will either be stained or marked, or it
will split off in drying, therefore care and attention are requisite;
even in preparing a piece of glass for the reception of the film of
collodion care is especially requisite, as the want of it cannot be
seen until after all the operations, therefore the labor and time are
not thrown away.

There are two methods of cleaning the glass plate: one quite
mechanical; the other is a mixture of the mechanical and the chemical.
Both are good. The second is perhaps the best, as it is simple and more
certain.

In the first method the glass, when new, merely requires polishing with
clean wash leather kept for this purpose.

The best way of doing this is on a flat board 24 by 18 inches, or
thereabouts, |22| covered with good American oil-cloth, glazed side
out. A plate laid upon this will not slip about when being polished.

Both sides and edges of the plate must be well cleaned, as one of the
most prolific causes of derangement of the silver bath is from organic
matter introduced by imperfectly cleaned glass plates.

One side of the plate, if gently rubbed with the thumb nail, will be
found smoother than the other, and is the suitable side for the support
of the collodion film; this side is polished with the leather until,
upon breathing gently upon it, the film of moisture is quite free from
marks or streaks, not only in the centre but at the sides and corners.

It is absolutely necessary that the plate be chemically clean all over,
else the film of collodion, upon drying, will split, and the negative
be spoilt.

When the plate is clean, an edging of India-rubber dissolved in
benzole, about an eighth of an inch wide, is run all round the edge,
by means of a small camel’s-hair brush tied to a stick, the end of the
stick being level with the point of the brush. The stick acts as a
guard against the brush going too far from the edge.

In the second method, the new glass plate is soaked an hour or two in a
mixture of 5 ounces of common spirits of salt (hydrochloric acid) in 80
ounces of water. After both sides of the plate are rubbed with a rag,
and well washed under the tap, it is put in a dish of clean water. When
all the plates have been so treated, they are taken out singly, again
well rubbed on both sides with another rag, and well washed; then the
smoothest side having been selected, it is twice flooded with a mixture
of albumen and water, draining the surplus into the sink each time of
flooding. The plate is then placed upon a rack to drain and dry; the
drying should be effected in a current of hot air freed from all dust.

The albumen mixture is composed of the white of one egg well beaten,
then diluted with 40 ounces of water and ten drops of liquor ammonia
added, and again beaten. It must then be very carefully filtered
through cotton-wool, and used as above.

In placing the albumenized plates upon the drying rack, care must
be taken to face the coated sides all one way, as when dry there is
nothing to indicate to the eye which is the back and which the front.

The albumenized plates, when dry, should have the backs cleaned with a
cloth or a leather before using, so as to clear away any albumen which
may have adhered during coating. |23|

Albumenized plates stored in a dry place will keep good for months,
_and do not require any edging with India-rubber_, as the most horny
collodion film will not split off an albumenized plate.

Glass plates that have been used, and not varnished, are freed from the
films by being immersed in a mixture of hydrochloric acid and water for
a few hours, then washed under the tap, well rubbed with a rag, and
put into clean water, from which they are taken singly and coated with
albumen; or they may be allowed to dry, and are then polished by means
of the wash leather.

Negatives that have been varnished are cleaned by first immersing in
a hot solution of common washing soda until the film comes off, then
wash them under the tap, rubbing well with a rag, then immerse them in
the acid solution so as to neutralize the alkali. Finally they may be
treated as above.

The films that are removed from the glass plates must not be thrown
away, but should be carefully collected, dried, and sent to a refiner
with the other silver waste; a good plan for saving these films, and
at the same time keeping the acid and soda solutions clear of them, is
to filter each solution occasionally through an old felt hat suspended
conveniently over the tanks, using one for each of the tanks.

The polishing of the glass plate must not be done in the dark-room,
or the crop of comets, spots, etc., upon the negatives will be
exasperating in the extreme; let this operation be conducted in a
clean, quiet corner of the studio, where no other operation will
disturb, and where the fluff from dusters and leathers will not
interfere with anything else.

|24|

CHAPTER III.

PHOTOGRAPHIC MANIPULATIONS.

The chemicals being prepared, they must be placed in the dark-room; the
collodion bottle should be placed on a convenient shelf close to the
door, and on a handy peg hang a broad camel’s-or badger-hair brush, for
dusting the clean plate just previous to coating it with collodion; the
brush must not be used for anything else upon any pretence whatever.
The silver bath must be kept, both in use and out of use, in some
convenient corner, where there is no risk of getting any other chemical
splashed into it. For a bath holder a deep 15 by 12 porcelain or papier
maché dish, with a wooden or stout cardboard lid, should be provided,
and this dish must always be thoroughly washed, and wiped dry with a
clean damp leather (kept for the purpose), both before use and after
pouring the silver solution back into its bottle or jug. Or, if the
upright form be preferred, be sure and have it large enough.

The developer should be placed on a shelf, on the right of the sink,
the developing cup close by.

The fixing or clearing solution should be kept in an upright bath of
glass, porcelain, or ebonite.

The intensifier No. 1 may be kept in a flat dish, or in an upright
holder, at discretion; but if in a flat dish, the solution should be
poured back into its bottle, after each day’s work.

Keep the intensifier No. 2 in a stoppered bottle close to the sink.

The water varnish also is kept in a bottle or jug.

On a shelf close to the collodion, the polished or albumenized plates
may be stacked, with the clean or prepared side facing the wall.

A pneumatic holder for attaching to the back of the plate during the
operation of coating with collodion will be found very handy.

Of course, it is thoroughly understood that there is a sink in the
dark-room, and a good water supply is indispensable.

Then, again, the window through which the light is transmitted, must
be |25| covered with a non-actinic medium, such as two thicknesses of
golden fabric, or one of canary medium; do not stint the amount of
light, but have as much as possible, so long as it is non-actinic.

No arbitrary plan for the dark-room need be followed, but the novice
will find the annexed plan useful to him in contriving for himself. It
is self-explanatory.

[Illustration: Fig. 2.]

Everything being in readiness, we will now proceed to make a line
negative, reserving a description of half-tone work to follow.

To begin: wash the bath holder thoroughly, and wipe it dry, then pour
into it sufficient silver solution to make the depth about half an
inch; dust the inside of the cover, and put it over the dish; now take
a clean glass plate, if it be polished, see that it is edged with
India-rubber, and if albumenized, be sure and clean the back—and attach
it to a pneumatic holder; then with a broad camel’s-or badger-hair
brush (kept for this purpose only) remove any particles of dust,
back and front; now hold the plate in a horizontal position and pour
upon it, toward the right hand corner furthest away from the body, a
little more collodion than it is judged will be sufficient to cover
it; let the collodion run to the corner, then incline the plate to the
left, and the collodion will run into the upper left-hand corner. Now
by inclining the plate toward the body the collodion will flow into
the lower left-hand corner, and thence it is guided into the funnel
placed in the bottle prepared for its reception; during the time that
this surplus is draining, the plate must be gently rocked sideways,
so that the lines formed by the collodion, in draining, are merged,
leaving the film quite homogeneous. As soon as the collodion ceases
to drip, release the plate from the pneumatic |26| holder, and touch
the lower ridge of the collodion; if it is quite set, close the door
of the dark-room, remove the lid from the bath holder, then—holding
the plate in the left hand—with the right hand raise the end of the
bath holder, as far as is possible without risking any of the silver
solution running over the end of the dish resting on the bench; now
lay the plate (with the collodion side up) on the bottom of the dish,
then drop the plate into the solution, and, at the same time, lower the
end of the dish held up by the right hand, which will cause the silver
solution to flow in one even wave over the collodionized surface. This
operation must be done with dexterity, as if the silver solution does
not flow in an even wave the film will be marked, and, in the case
of a half-tone negative, the image will be spoilt. Therefore, it is
necessary to see that the plate and dish are lowered simultaneously, so
that the solution goes over the collodion film in one steady wave. If
the upright bath holder be used, the plate is placed upon the ledge of
the dipper, and lowered slowly and steadily into the solution.

The plate will require an immersion of about three minutes for proper
sensitizing, and this interval—the bath being covered up to prevent
the access of white light—may be utilized to give the final adjustment
to the camera, and to see that the drawing or print to be copied is
properly in focus.

Use a medium diaphragm in the lens for focussing, and examine the
image all over before deciding that it is sharp. Focus by preference
about halfway between the centre of the picture and the edges, and
then, after moving the rack to and fro until the proper sharpness is
obtained, take out the diaphragm and substitute the smallest sent out
with the lens; or if the picture to be taken be small and from a large
original, then the second, or third, smallest diaphragm may be used.

Now remove the focussing screen from the camera (note that the ground
side of the glass has been next the lens) and place the cap upon
the lens; close the door of the dark-room, open the dark slide, see
that the proper carrier is in it, then raise the plate from the bath
slowly, using a silver-wire hook for the purpose. If the solution flows
evenly over the film, the plate is ready; but if, on the contrary,
the solution flows greasy, then again lower the plate and rock the
dish gently for a minute or two. The film being fully sensitized, the
plate is carefully lifted out of the solution, both hands holding
the plate in such a manner as to avoid touching the film; allow the
solution to drain from the plate as much as possible, then lean the
plate against the wall, the lower end resting upon a pad of clean
blotting-paper, so as to catch any further draining; |27| now with a
pad of blotting-paper or papier-joseph wipe the back of the plate as
dry as possible; this will prevent stains, and keep the dark slide from
rotting by the action of the silver solution.

The plate being drained, lay a piece of thin filtering paper in each
lower corner of the carrier, so that the plate will rest upon the
filtering paper, which will catch any further drainings from the film,
and be a safeguard against stains.

Now lay the plate face down in the carrier of the dark slide, close the
door, and fasten it.

The dark slide is now carried to the camera, and inserted in the
grooves previously occupied by the focussing screen, taking care that
the sliding shutter is next the inside of the camera; when pushed quite
home, cover the back with the focussing cloth; pull out the shutter,
when the plate is ready for the exposure.

The time of exposure will vary very much with the time of the year, and
with the amount of light falling upon the object being photographed.
The exact time can be found out only by actual practice, but the
operator, in time, by observation, will be able to guess it pretty
correctly.

In taking the cap off the lens, be sure that the camera is not shaken,
else the picture will be spoilt.

The exposure being made, close the sliding shutter, remove the slide
to the dark-room, and close the door; lay the dark slide (with sliding
shutter down) upon the bench, open the back shutter, and, placing the
pneumatic holder in the centre of the plate, lift it out of the carrier.

Take the plate to the sink, and holding it face up, in the left hand,
take the developing cup in the right, and, with a quick motion,
pour over the plate sufficient developer to cover the whole film;
the developer must go all over the film in one even wave, for any
hesitation in this will result in a stain; pour upon the film only
sufficient to cover it, and be careful to spill as little as possible
into the sink, or else the image will be thin, on account of the
absence of free silver washed off by the wave of developer.

Now rock the plate gently, so as to keep the developer flowing to and
fro over the film (but keep it there, don’t spill it off) and the
image will soon appear, faint at first, but growing gradually darker,
the black lines of the drawing being white and the white paper black.
If the development be continued too long the lines will eventually
be veiled; therefore, as soon as the finest details are out and well
defined, place the plate under the tap and allow |28| the water to
well sluice the film all over; as soon as it is properly washed, which
can be seen by the water flowing evenly over, without greasy looking
lines, hold the negative up in front of the window, and examine for
spots or stains. If there be any present that at all interfere with the
picture, at once reject the negative, placing it in a pan filled with
water, to be washed off at leisure. Then start afresh.

The negative being satisfactory, give it another rinse under the tap,
and place it in the cyanide bath, where the unaltered iodide will
speedily be dissolved. Then it is withdrawn, and well washed under
the tap. Whilst the water is washing over the front, rub the back
with the fingers or a sponge, and then turn the plate over and allow
the water to wash the back also. It is now ready for immersion in the
intensifier No. 1, where it remains until the film is bleached almost
white. Then it is thoroughly washed, drained, and flooded with a small
quantity of intensifier No. 2, which will at once turn the film to an
intense black, or if the action does not penetrate through to the back
of the film, continue the application until it does; again wash, then
place the negative on a rack to drain. When the water ceases to drip,
flood the plate twice with the filtered water varnish. Then place the
negative on the rack to dry. When dry, it is ready for printing on
zinc. The negative may be varnished with a benzole varnish, sold by
the dealers under the name of positive or ferrotype varnish. Negative
varnish may be used, but unless very thin it is apt to be sticky and
render the negative easily marked by the heavy pressure it is subjected
to in the printing-frame.

Now lay the finished negative face down upon a piece of clean white
paper, when, if it is a good one, all the details of the original will
show through, clearly and distinctly; but if any of the details are
missing or veiled over, the negative will not do, and another must be
made.

This process does not always work satisfactorily, but with care and
cleanliness no serious fault should arise.

Sometimes the bath may give what are called foggy images, which are
indicated by a veil over the lines. These can often be wiped off with
a pledget of cotton-wool. The addition of half a drachm of nitric acid
to the eighty ounces of bath solution, thorough mixing, and a rest for
a few hours, will end this difficulty. If the dark-room window be not
of the proper color, fog will ensue; therefore, the non-photographic
experimentalist had better call in the aid of a professional
photographer in case of any difficulty in getting clear negatives.

_Wilson’s Photographics_ will be a profitable investment, as it was
published |29| before the advent of dry-plate photography, when the
wet process reigned supreme.

At the end of each day’s work the silver solution should be carefully
poured into the jug or bottle, and allowed to stand all night; then in
the morning, just before using, it should be filtered. The dish also
must be carefully washed out and put away in a corner where it has no
chance of being soiled.

Such are the manipulations necessary for the production of a negative
from a line subject—_i. e._, a drawing in black and white, in which the
whole of the picture is obtained by means of lines, or stipple, or by
cross hatching. Flat washes of color not being permissible, all effects
of half tones, etc., are obtained by lines, either thicker, or thinner,
or closer, or further apart. Such a negative is available for printing
from, direct upon zinc, in either albumen or in bitumen, for etching
into relief, or for printing from as a lithograph.

THE USE OF GELATINE DRY PLATES IN PHOTO-ENGRAVING.

For making negatives for collographic printing either direct or by
transfer, gelatine dry plates may be used with as much certainty as the
wet collodion, so long as the operator can produce a result giving all
the gradations of tone, from the deepest shadow to the highest light;
and as there are so many excellent brands of plates in the market,
it would be worse than useless to name any brand here as having any
distinct advantage over the rest, more especially as the brand that
the writer would be inclined to name, would perhaps, by the majority
of readers, be classed as a plate that they could not work. This being
so, for half-tone negatives, the author leaves the choice of the plate
and the manner of working to the operator, contenting himself with
saying that the criterion of suitability of a negative for yielding
good results by any of the processes treated of in this book, leaving
out of the question entirely negatives for line work, etc. (treated of
in Parts I., II., and III.), is the same for giving soft, delicate, and
brilliant prints, either in platinum, carbon, or on albumenized paper,
resting assured that a negative yielding a hard black and white, or a
dirty flat print, by any of these three methods, will not give results
any different in collographic or transfer methods.

For line work negatives for printing upon zinc, for etching, or for
transfers to stone, ordinary gelatine dry plates are not useful, as
it is almost impossible to get that freedom from veil over the lines
that it is absolutely necessary to have; here the wet collodion is best
as it is simplest, easiest, and cheapest. |30| Still there are times
when the most ardent wet-plate worker is obliged to confess that the
process has its shortcomings, most especially in dull weather, when it
is necessary, to get the result required, to give exposures from thirty
to sixty minutes; then, what with the plate drying and the want of
pluck from the bad light, it is impossible to get a result suitable for
the work. In this case the plate called the “Process” plate is a great
boon. It is fairly rapid, and gives intense negatives, without veil on
the lines.

For making transparencies same size of original negatives, the best
plan is to place a large sheet of white paper in front of the copying
camera, and rack the lens out of focus, taking care that the white
sheet of paper is sufficient to illuminate the full size of the plate.
Then in the dark-room place the negative in the carrier of the dark
slide, film side up, and carefully dust the surface (also seeing that
the back of the negative is clean) with a clean camel’s-hair brush;
dust also the film of a gelatine dry plate, and place it face down
upon the negative, close the slide, and insert it into the grooves of
the camera and expose to the light reflected through the lens from the
white sheet of paper for from five to twenty seconds, according to the
density of the negative and the intensity of the light; close the lens
and the shutter, and remove it into the dark-room for development.

By exposing a plate in this manner there is a far better chance of
getting absolute contact between the two plates, as the rays of light
are parallel.

For making transparencies for printing upon copper-plates, first of all
make a grained negative the proper size, then when this is varnished
and touched up, make from it as above a transparency upon a gelatine
chloride dry plate, by which process it is more certain to get a
suitable result for the process than on a gelatine bromide dry plate.

No formula will be given here for developing these gelatine chloride
plates as each packet has full instructions for development which must
be followed implicitly.

For developing gelatine bromide dry plates for negatives, or for
transparencies, the following, a modification of the Ilford formula,
will be found better than using formula where the ammonia and bromide
are mixed together.

_Solution No. 1._

Pyrogallic Acid 1 ounce.
Meta Bisulphate of Potash 1 ounce.
Bromide of Potassium 1 ounce.
Water 80 ounces. |31|

_Solution No. 2._

Liquor Ammonia 1/2 ounce.
Water 10 ounces.

For a normal exposure equal parts of these are mixed just before using,
and for an uncertain exposure begin with two parts of No. 1, one part
of water, and one part of No. 2.

THE REPRODUCTION OF NEGATIVES.

For the production of suitable collotype prints, the first
consideration is the negative, from which the printing surface is to
be made. The requirements are, a negative in which all the half-tones,
both in the lights and in the shadows, are reproduced in their proper
gradations; the lights must not be too dense, or the shadows too clear;
the blackest portion of the negative must be that part representing
the highest light, and the only clear glass, that which represents the
deepest shadow; these negatives may be either wet collodion, or on
ordinary gelatine-bromide plates and reversed—_i. e._, the mirror must
be used behind the lens. If it is desired to produce a collographic
block from a negative already in existence, and which may not be
retaken, then it will be necessary to make another negative. This may
be done in many different ways; but whichever way is adopted, the first
and most important step is the production of a transparent positive.

This transparent positive may be made on an ordinary gelatine-bromide
plate, or on a gelatine-chloride plate, and then from the transparent
positive a negative is made by transmitted light (in the enlarging
camera), either the same size, reduced or enlarged in size; or instead
of using this class of transparency, by far the finest results can be
got by making the transparency in carbon tissue, which can be used for
both transmitted light, for enlarging or reduction in size, and it can
also be used for contact printing, when the reproduced and reversed
negative is required to be the same size as the original.

On page 29 directions are given for the manipulations when gelatine dry
plates are used, so here we will confine ourselves to the production
of negatives from the carbon transparency. First of all, procure some
carbon transparency tissue, ready sensitized, cut this into sizes at
least half an inch larger all round than the negative, then cut a brown
paper mask to fit all round the negative, and to protect the margin
of tissue from the action of light; this acts as a safe edge to the
tissue, enabling it to adhere to the glass support during the operation
of development. If it is only intended to reproduce a portion of the
|32| original negative, the safe edge may be made by putting the mask
just round that portion of the image, but if the whole of the negative
is required, put it in a printing frame with a plate glass front, fix
the brown paper mask outside the negative, then place the sensitive
carbon tissue the black side next the negative film, and put in the
backing, and back, and fasten it up. Next expose it to the light for
four or five times the time requisite to get an ordinary silver print.

The carbon tissue having been exposed to light for the proper time, it
is taken into the dark-room, the edges are turned up so as to form a
dish, and pinned upon a small board; it is now coated with thin plain
collodion, the surplus being poured into a bottle kept for the purpose,
and the board gently rocked to and fro, so as to prevent the collodion
running in ridges, or streaks. Now allow the collodion to dry, then
place the coated and exposed tissue in clean cold water until it is
quite limp, then slide underneath it a gelatinized glass plate a little
larger all round than the tissue, bring the gelatinized surface of the
glass plate and the collodionized surface of exposed tissue in contact
under the water, taking great care not to abrade the collodion; then
lift the two out and lay the glass down upon a bench, and cover it over
with a piece of thin India-rubber, or mackintosh, or oil-cloth. Hold
the cover firmly on the bench with the left hand; with the right use a
strong squeegee vigorously. That will expel all the water from between
the two surfaces (collodion on the tissue, and gelatine on the glass),
and so bring them into absolute contact; now remove the cover, lift the
plate and examine the tissue through the glass, and if there are no
air-bells between the two surfaces the operation has been successful;
but if air-bells are present, _at once_ plunge the plate into cold
water, strip off the tissue, and try again, but be careful to be quick
about it, or there is a risk of the tissue absorbing too much water, in
which case great difficulty will be experienced in getting it to lie
flat upon the gelatinized glass.

The gelatinized plate upon which the exposed and collodionized tissue
is mounted is prepared as follows: Glass plates free from scratches and
stains, are placed in a weak mixture of hydrochloric acid and water,
and rubbed with a clean rag until free from grease and dirt; they are
then washed under the tap, and whilst wet are covered with:

Gelatine 1 ounce.
Water 20 ounces.
Bichromate of Potash 15 grains. |33|

Soak the gelatine in the cold water until it is soft, then melt at
gentle heat, add the bichromate, and when dissolved, filter, and coat
the cleaned plate two or three times, throwing the surplus away each
time of coating; now stand the coated plate on a rack to dry. Any
quantity of these plates may be prepared at a time, and used when
required. When all the batch has been coated, the rack may be removed
into a warm corner, free from dust, until the plates are dry, then
expose the plates to the light for at least twenty minutes, when
they are ready for use for mounting the exposed and collodionized
transparency tissue upon.

After the tissue is mounted upon the glass plate, it is allowed to
stand a few minutes, then it is placed in a dish containing hot water
(100° F.), and as soon as the tissue compound shows signs of dissolving
by exuding from under the paper, lift the paper away, then rock the
dish, and, if necessary, add more hot water; then raise the plate and
gently lave it with the hot water, until the whole of the soluble
pigmented gelatine is washed away, leaving a transparent positive on
the glass, which merely requires washing under the cold water tap, and
drying, to be finished. Now examine it closely, and if it contains the
whole of the details in the negative, and is free from dust spots, it
may be put away to dry, but if underexposed, or overexposed, or marred
by spots not in the original, then another must be done; but if care is
taken to dust the surface of the tissue, and the film of the negative
with a camel’s-hair brush before printing, and before collodionizing,
and also to see that both the collodion and the gelatine mixture are
properly filtered, and that the water in which the coated and exposed
tissue is soaked is free from dirt, then there will be no difficulty in
getting a perfect transparency.

The transparency being obtained, if it is desired to make a negative
larger or smaller than the original, the transparency is placed in the
enlarging camera with the carbon film inside, and the negative made the
requisite size, either on a dry plate or on a wet collodion plate.

If a negative the same size is required, the transparency is placed
face up in the carrier of the dark slide, and the surface dusted; then
take a dry plate, and having also dusted its film, place it face down
in contact with the transparency, then close the dark slide and remove
it to the camera, which should be previously adjusted opposite a large
sheet of white paper; now put in the dark slide, draw the shutter, and
expose to the sheet of paper, and develop as directed on page 30.

By exposing in this manner, instead of direct to the light (day or
gas), the |34| rays projected through the lens fall upon the dry plate
quite parallel, so securing sharp negatives.

In making reversed negatives for collographic printing when wet
collodion is used, it is not absolutely necessary to use the mirror, as
they may be made upon polished glass (_i. e._, not albumenized) dried,
then coated with gelatine, again dried, and stripped.

Some brands of dry plates can also be stripped, by first of all, after
drying, coating them with India-rubber solution, then with collodion,
and soaking in dilute fluoric acid; but great care and patience must
be exercised, the preliminary trials being made upon negatives of no
particular value.

STRIPPING COLLODION FILMS.

Negatives made by the wet collodion process can be easily stripped
from the glass support, and in such a condition are extremely handy,
especially for printing on collographic plates, or on zinc or copper,
as, the film being flexible, contact is more easily secured.

When it is intended to strip the film, the glass plate must be
polished, _not albumenized_, and after the negative is dried, strips
of thick paper are pasted along the four sides of the negative, with
starch, or a solution of gum tragacanth; the negative is then placed
on a levelling stand and a sufficient quantity of the following warm
solution of gelatine is poured upon the plate (which should be slightly
warmed first) and spread all over it by means of a glass rod:

Gelatine 2-1/2 ounces.
Sugar 1-1/2 ounces.
Water 20 ounces.

Soak the gelatine in the water until soft, melt by gentle heat, then
strain through two or three thicknesses of fine muslin, and pour upon
the plate, using three ounces for a plate 12 × 10; more or less, in
proportion for different sizes. The plate must be allowed to stay upon
the levelling stand until the gelatine has quite set, then put it on a
rack to dry, in a current of cold air, for if heat be used the gelatine
will melt.

When the gelatine is _quite dry_, pass the blade of a penknife all
around underneath the strips of thick paper, when the negative film may
be lifted away from the plate.

In this condition the negative may be stored away without risk of being
broken, the only condition being, it must be kept free from dampness.
|35|

Another plan of stripping is to coat the dry negative with a thick
solution of India-rubber in benzole, and allow it to dry on a levelling
stand; then coat with a thick plain collodion, to which a few drops of
castor oil have been added. When the collodion film is quite dry, place
the plate in a dish of clean water, strip off the film from the glass,
then place the film between sheets of clean blotting-paper to dry, or
it may be allowed to dry on the plate.

Old collodion negatives that have been varnished may be stripped, but
it is rather a risky operation, and should never be attempted until a
really good carbon transparency has first been obtained.

The first step will be to remove the varnish, which is effected by
soaking the plate in

Alcohol 1 part.
Ammonia 1 drachm.

until all the varnish is removed, then rinse in alcohol, wash well
under the tap, dry, paste slips of brown paper around the margin, and
finally level and cover with the warm gelatine, dry and strip.

THE REVERSING MIRROR.

The mirror is a piece of perfectly plane glass, coated on the surface
with a thick film of pure silver, and highly polished. This silvered
glass must be mounted in a mahogany box, and fitted on the front of the
camera, the lens being fitted in front of the mirror, see Fig. 1. This
mirror is placed in grooves at an angle of forty-five degrees from the
axis of the lens. So situated, it receives the image projected by the
lens, and reflects it on the focussing screen, or sensitive plate in
the camera. By this means a negative is obtained, which, when looked
through with the film between the operator and the glass, will present
the image in its proper position, whereas, if the lens be used without
the intervention of the mirror it will be necessary to have the glass
between the eyes and the film, to get the image in its proper position,
and as the generality of photographic negatives are taken without the
intervention of the mirror, they are called ordinary negatives in
contradistinction to those made through the mirror, which are called
“reversed” negatives.

The silver surface of the mirror requires great care and attention to
preserve its lustre. If tarnished, it will make the exposure in the
camera longer, besides which, the cost of resilvering is too great to
allow of the surface being spoiled through carelessness. |36|

At the end of each day’s work, remove the mirror from the box and warm
it in front of the fire (not over a gas flame) just slightly, then wrap
it carefully in a piece of fine velvet, which has also been previously
warmed, then wrap it up in a piece of India-rubber or macintosh cloth,
and put it in an air-tight box; by doing this, the mirror, if well
silvered at first, will last for a year or two.

If the surface should become tarnished, get a square of very fine
chamois leather, and place in the centre a pellet of cotton-wool; then
gather up the leather and tie the wool in the centre, making a small
globe about an inch and a half in diameter; now warm the mirror, and
after dipping the leather globe into fine rouge, proceed to polish
gently with a quick circular motion, using little or no pressure—take
care in doing this that the mirror, the leather, and the rouge are
quite dry, else the silver coat will come away—_verb sap_.

In purchasing a mirror be sure and get it large enough to take the cone
of rays from the lens it has to be used with; for a lens three inches
in diameter, the plane mirror should measure about 8 × 3-1/2 inches.

The box to hold this mirror should be made square at the side, fitting
into the rabbet of the camera front, so that when objects are to be
photographed that will do better lying on the ground than when fixed
against the wall, the mirror can be placed to look down upon the object.

For silvering the glass, one cannot do better than to quote the
directions for working Common’s process given by Major Waterhouse in
the _Photographic News_.

“The solutions recommended by Mr. Common are three:

(1) Nitrate of Silver 1 ounce.
Distilled Water 10 ounces.
(2) Caustic Potash 1 ounce.
Distilled Water 10 ounces.
(3) Glucose 1/2 ounce.
Distilled Water 10 ounces.

The above quantities are suitable for 250 square inches, consequently,
an ordinary copy mirror 8 × 6 would require rather more than two ounces
of each solution, and other sizes in proportion.

The caustic potash and distilled water must be quite pure. Ordinary
caustic potash will not answer at all. The best to use is known as
_pure by alcohol_.

The glass surface to be silvered is carefully cleaned with strong
nitric acid, applied, as recommended by Mr. Browning, with a Buckle’s
brush, then well |37| washed in clean water, and after rinsing with
distilled water, laid, face downward, in a dish of distilled water
until wanted.

Before cleaning the glass, it will be necessary to arrange for
supporting it face downward in the depositing dish, so that the surface
to be silvered may be quite horizontal, and just below the level of the
fluid, which should be about half an inch above the bottom of the dish.

I have generally used a large cork, about four inches in diameter,
cemented to the back of the plate, and fitted with three strings, by
which it could be suspended in a level position and adjusted to any
height by winding the string over a roller placed at a convenient
height above the dish. When this arrangement is not available, I fix on
the back of the plate two ordinary wide-mouthed bottle corks of equal
thickness, in the positions shown in the figure, and to these corks
attach thin slips of bamboo running transversely across the plate, and
of sufficient length to rest on the sides of the dish, thus:

[Illustration: Fig. 3.]

The slips of bamboo give the arrangement a certain amount of spring, by
which the height of the plate can easily be regulated, by putting on
weights until the surface of the plate is just below the level of the
fluid in the dish.

To prepare the silvering solution: A sufficient quantity of the
silver solution, No. 1 (two ounces), is put into a perfectly clean
glass. Ammonia is dropped in until the precipitate first formed is
just redissolved. The same quantity of potash solution, No. 2, as of
silver is now mixed in, and the precipitate again dissolved by ammonia.
A little more silver solution is then added to produce a distinct
turbidity, and distilled water to make up the quantity necessary to
fill the depositing dish to about three-eighths or half an inch, and
the mixture is then filtered through cotton into another clean glass
vessel.

The same quantity (two ounces), of filtered solution of glucose, No.
3, as was taken of silver and potash, is now mixed in, and the whole
is poured into a depositing dish (which should preferably be of glass,
well cleaned with nitric acid).

The glass plate is then taken out of the distilled water and laid
face downward on the silvering solution, being supported, as before
described, just above the surface, so that the solution does not cover
its back.

Mr. Common places the requisite quantity of distilled water in the dish
in |38| which the mirror has been remaining face downward, and then,
having lifted the mirror up, pours in the undiluted silvering solution,
together with the glucose solution, stirs well together, and then
carefully lowers the mirror again into the dish.

Almost immediately after the immersion of the plate, the silvering
action begins, and, if things are going on well, a brilliant reflecting
surface will be seen at the back of the plate, and in forty minutes,
or even less, a good deposit of silver will be obtained. It is usually
recommended to stop the action as soon as the silvering fluid appears
clear and free from turbidity, but it is not always easy to see this.

After silvering, the plate is well washed, finishing with distilled
water, and dried off quickly. A slight cloudiness of the surface may
appear, and must be removed by polishing before the mirror can be
used. It is better to allow the mirror to remain a day or so before
polishing, in order to harden the coating.

To polish the plate, it should be slightly warmed, and perfectly dry,
and rubbed very gently in small circles with a piece of very soft and
dry chamois leather, afterward using a little jewellers’ rouge.

Mirrors should always be kept in a dry place, and will require
repolishing from time to time.

|39|

CHAPTER IV.

APPARATUS FOR PRINTING UPON ZINC.

A suitable negative (the subject being in line, _not half tone_) having
been obtained, the next stage toward producing a relief block is to
make from that negative a print in ink upon a sheet of zinc. To do this
a sheet of polished zinc is first of all subjected to the action of a
solution of nitric acid, alum, and water. It is then thoroughly washed,
placed in a machine called a whirler, then coated with a solution of
albumen (white of egg) and bichromate of potash; this coat or film of
bichromated albumen should be dried over a spirit lamp.

The negative is then placed, face uppermost, in a printing-frame, the
coated side of the zinc in contact with the face of the negative. The
negative is now exposed to the action of light.

The exposure being complete, the frame is taken into a room lighted
by yellow light, gas, or lamp-light, the zinc plate is removed, and
its surface covered with a thin film of transfer ink, by means of a
type-printer’s roller; then the zinc plate is immersed in clean cold
water and the image developed by gently rubbing it with a pledget of
cotton-wool.

POLISHING THE ZINC.

Zinc plates suitable for photo-engraving can be obtained either in
large sheets, or cut to size as ordered, and, when new, require
polishing with a damp rag dipped in levigated pumice powder—_i. e._,
pumice powder washed in water, so as to get rid of all grit.

Lay the plate upon a board covered with muslin and polish with a
“from-and-to” the body motion, not circular; do not use a great deal
of pressure, the object being to get the plate highly polished with a
perfectly smooth surface.

Plates that have been printed upon, and are not satisfactory, may be
cleaned and repolished.

Plates that are scratched require polishing with emery cloth. Scratches
interfere with the picture. |40|

To remove scratches, sprinkle the face of the plate with turpentine,
then rub with a piece of FF emery cloth stretched over a carpenter’s
cork-covered rubber. Use the same motion, to-and-fro, until all the
turpentine has evaporated and the surface of the zinc is polished. If
the scratches are removed, the plate is ready for use, but if not,
then the operation must be repeated. If the scratches are too deep for
emery cloth alone, first use a piece of fine pumice stone, followed
by snake stone, pumice powder, rotten-stone, and rouge. Too much care
cannot be taken with the zinc plate at this stage, for, after the block
is etched, if it is discovered that the plate has not been properly
polished, all will have to be done over again, entailing a loss of
time, labor, and materials.

Remember, that no matter what polishing agent is used, the plate must
be polished with a to-and-fro from the body motion, not a circular
motion such as is usual in polishing metal.

GRAINING THE PLATE.

The next operation is to give the plate a slight tooth so that the
sensitive solution will flow evenly over the surface. Do this by
removing all traces of grease.

This graining is done in a wooden tray, 24 inches by 18 by 6, lined
with asphaltum or gutta percha and mounted upon rockers; it is quite
necessary that the graining tray be of large size, as if only a little
larger than the plate the returning wave of acid water will mark the
edges of the zinc.

Into this tray pour a quart of clean water, and add one drachm of
nitric acid and one ounce of a saturated solution of common alum. Place
the plate in this, face up, and commence rocking it at once or else
the acid will mark the surface, and it will require repolishing; rock
slowly for five minutes, during which time the polished surface will
give way to a fine matt, like fine frosted silver. Now remove the plate
and rinse it under the tap, rubbing it gently with a fine sponge, or a
pledget of cotton to remove the scum or deposit formed by the acid. The
surface at this stage should be quite smooth; if it is at all rough,
the acid is too strong, and the solution must be diluted with water; if
the action of the acid is very slow, then a little more must be added;
but it will only be necessary to add more alum when the plate is a
bluish color instead of being a pearly gray.

A drop or two of acid will be required each time plates are to be
grained.

In rubbing with sponge, or a pledget of cotton when under the tap, care
|41| must be taken not to scratch the surface of the zinc, or else it
will need repolishing.

COATING THE PLATE WITH SENSITIVE ALBUMEN.

If the solution of albumen was poured over the plate and drained and
dried, the film would be too thick at the bottom and too thin at the
top; it is, therefore, necessary, to insure an even film of sensitive
albumen, to subject the plate to a quick circular motion, so as to
spread the film of albumen evenly, and to get rid of the surplus
solution. This is effected by placing the grained zinc in the jaws of
an instrument called a whirler and made as follows:

Two pieces of wood, each half an inch thick, twelve inches long, nine
inches wide at one end, and six inches at the other; upon the narrow
end of one piece fix four screws, a piece of iron the shape of a ┻,
the top end of which is shaped to fit into the socket of a carpenter’s
brace (which must have the centre handle revolving, not fixed); the
cross piece must be flat, and pierced with four holes, countersunk to
admit of stout screws.

Place the two pieces of wood together, the ┻ piece between the two,
and with a piece of stout leather hinge the two together, nailing the
leather not only on the outside, but upon the top also; now screw a
narrow batten on each of the pieces, about an inch from the widest end,
to keep the wood from warping.

Four inches from the top (the hinge being the top) bore a hole through
both pieces, and pass through a couple of strong leather laces; by
one end fix these on the outside of the cheek to which the iron ┻ is
screwed, and on the outside of the other cheek, seven inches from the
top, hinge a piece of wood (so as to fall toward the bottom) 5 inches
by 2 by 1/2; and in the centre of the batten screwed on to prevent
warping, fix a broad-headed nail or a turn-button, over which the free
end of the leather laces can be passed.

Now about half an inch from each end drive through the wood, six or
eight wire nails one inch long in a line, and so that the points
project on the inside of each cheek. Next fix the top of the iron into
the socket of the brace and the whirler is ready for use.

To use this instrument, lay it upon the bench, raise the upper jaw,
place the grained zinc behind the teeth (face out) close the jaw,
and after seeing that the face of the zinc is close up to the teeth,
tighten the shoe lace, pass it over the hinged piece (which is lying
down close to the cheek), and around the batten with two or three
turns, then pass it back and tie the loose ends around the iron shank
at the top; then raise the hinged piece, which by straining on the |42|
leather laces will cause the jaws to grip the zinc plate tight and
hold it in position. (See Fig. 4.)

[Illustration: Fig. 4. The Whirler.]

Now lift up the whirler from the bench, grasping the handle of the
brace firmly in the right hand. Hold it at arm’s length, and by a
series of quick jerks set the plate revolving. This will require a
little patience to do evenly and rapidly, but with practice it will
become quite easy.

The plate is coated twice, whirling it after each application of the
sensitive mixture. The whirler is then laid upon the bench, and the
hinge piece let down. This relaxes the strain upon the leather laces,
and allows the jaw to be lifted and the plate removed.

An inverted revolving egg-beater may be made to serve for the same
purpose.

DRYING THE COATED ZINC.

The film of albumen now requires drying, which should be done over a
spirit lamp. The best form of lamp is one of the small pocket spirit
stoves sold by ironmongers, and having the three supports for a kettle
cut away. The zinc is held over the flame and kept in constant motion,
so as to dry the film as quickly and evenly as possible; no fear need
be felt at applying too great a heat so long as the metal can be held
comfortably in the fingers. When dry, the plate is ready for printing
upon.

For drying large plates, two or more of these stoves would be required,
but it is very easy to extemporize a suitable arrangement, by laying a
large pad of cotton saturated with spirits of wine in a tin dish, and
setting it on fire; by this means a stove of any desired dimensions can
be prepared quickly. To extinguish such a flame, cover it with a large
sheet of zinc.

It must be borne in mind that the film on the zinc is now very
sensitive to |43| light, therefore the preparation of the film must be
done in a yellow light, as must also the operation of placing it in the
printing-frame, inking up, and development; gas or lamp light may be
used, as the film is not sensitive to artificial light of a low actinic
power.

THE PRINTING FRAME.

The printing-frames used for this purpose must be of the box pattern,
fitted with stout plate-glass fronts, the cross bars behind being
fitted with wooden screws, instead of springs, as absolute contact can
only be obtained between the surfaces of the glass negative and zinc
plate by means of screw-pressure.

The front glass of the printing-frame must be kept perfectly clean, and
especial care must be taken that no grit be upon either glass, inside
the frame, or on the back of the negative, else the negative will be
broken.

TIMING AND EXPOSURE.

The time of exposure to light is measured by means of an actinometer,
which is simply an instrument in which is a strip of sensitive
paper, exposed under a graduated series of different thicknesses of
translucent paper, each division or gradation being distinguished by a
number, thus: No. 1 has only one thickness of paper over it; No. 2, two
thicknesses, and so on. But on account of the ever varying intensity
of the light, a screen actinometer that is reliable is almost an
impossibility. The best must be closely watched in a bright light, so
that the tints are changed evenly.

Johnson’s actinometer is very simple and handy; it consists of a
cubical box with two lids, the inner one serving to press the paper in
contact with the glass of the outer lid; the outer lid has a circular
opening with a narrow rectangular strip in the centre transparent,
the rest of the glass being covered with pigment the color assumed by
the sensitive paper after exposure to the light. When the strip of
sensitive paper inside has assumed this color, it is called one tint;
the strip of paper is then pulled forward, and another portion, quite
white is brought under the transparent portion of glass, and when the
light has turned that the color of the pigment, that counts two tints,
and so on. The paper used in the actinometer is ordinary albumenized
paper.

The exposure of zinc in the printing-frame under a good line negative,
will be about six or eight tints in diffused light, but in direct
sunlight the exposure may be timed by the watch, a suitable line
negative never requiring more than from three to five minutes. |44|

INKING THE EXPOSED ZINC.

The sensitive zinc having been exposed to light under the negative,
next cover the surface with a thin coating of litho-transfer ink, stone
to stone.

For this purpose we require a type-printer’s composition roller,
mounted upon a litho stock. This roller must be perfectly smooth and
cast in a solid mould, as the line along the side, formed by a split
mould would render it useless for inking up a zinc plate. A roller
eight inches long by five or six inches in diameter is a useful
size. We also require an inking slab, a palette knife, a bottle of
turpentine, with the cork cut so that the turpentine can be sprinkled
out without having to remove the cork, a tin of transfer ink, and a
linen cloth or two.

The inking slab may be made of smooth iron, or a suitable lithographic
stone is good.

|45|

CHAPTER V.

PRINTING ON THE ZINC IN ALBUMEN.

The negative being ready for printing, select a piece of zinc a little
larger each way than the picture, polish, then grain, and after well
washing it under the tap and gently rubbing it with a fine sponge, or
a pledget of cotton-wool, place it in the whirler; again rinse under
the tap, now invert the whirler and set it revolving; then examine the
surface of the zinc and see that there is no dirt on the surface, but
that it is quite smooth. If it is not, rinse it again under the tap,
and rub it gently with the sponge, and again rinse. This should quite
free the zinc from any deposit of dirt. Now whirl it so as to get rid
of as much as possible of the water, then pour over the surface of
the zinc sufficient to cover it, of the following solution (carefully
filtered through cotton-wool):

Albumen of one Egg.
Water 7 ounces.
Saturated Solution of Bichromate of Potash 1 ounce.

Place the white of egg in a bottle containing a lot of small pieces
of perfectly clean glass, then add the water and shake it well for a
minute; then add the solution of bichromate and again shake it well.
Now place a pledget of cotton-wool in the neck of a glass funnel, and
pass a few ounces of clean water through (if this is not done, there
will be difficulty in getting the albumen to filter); drain as much as
possible of the water away, and then filter the albumen into a clean
bottle; when all the solution has gone through, remove the cotton-wool
from the funnel, which well wash, then recharge with a fresh pledget,
pass some water through, and again filter the albumen solution through,
this time into a ten ounce glass-measure, which is to be used for
pouring from upon the zinc. The stem of the funnel should be long
enough to reach the bottom of the glass measure, so that the formation
of air-bubbles be avoided, which is impossible with albumen if the
funnel is not below the surface of the filtrate.

Of this, pour over the zinc sufficient to well cover the surface,
letting any surplus go into the sink; then set the whirler revolving,
coat again, and |46| again whirl; now examine the surface, and if it
is free from dust, spots, and air-bubbles, remove the zinc and dry it
over the spirit stove. But if either air-bubbles or dust be present,
wash them off under the tap, and begin again.

The film being dry, get the printing frame ready, see that the surface
of the glass inside is quite clean and free from grit, as also the back
of the negative, taking special care that the ridge of varnish which
often forms at the bottom of the negative be removed, as the slightest
inequality of surface will surely cause disaster directly the screws
exert their pressure.

Do not lay the negative into the frame flat upon the glass, but slide
it in from one side, so as to carry any dust away from the glass front
of the printing frame.

The negative being in the frame, film side up, lay the coated zinc upon
it, face down, judging the proper position and placing the zinc flat
down upon the negative; now put a piece of brown paper over the back of
the zinc, then place the back of the printing frame in place, fasten
down the cross bars and apply the pressure screws, evenly and gently.

Do not screw one side tight before the other has been touched, but
screw down so as to tighten all as evenly as possible.

Even pressure being applied, see that the front of the frame is clean,
and then expose to direct sunlight for five minutes. Remove the frame
to the dark-room, unfasten the cross bars and remove the zinc, taking
great care to avoid scratching its film against the film of the
negative.

After wiping the inking slab with clean linen place a piece of the
transfer ink, about the size of a small bean, upon the upper corner,
sprinkle this with a little turpentine, and mix them with the palette
knife until they are of about the consistency of printing ink.

Now with the palette knife spread some of this mixture as far as
possible over the inking slab, and then distribute it with the
composition roller. Roll to and fro, across and diagonally, until
there is a thin, even coating of ink all over the slab (not touching
the corner where the ink was mixed with the turpentine) and upon the
roller; if the mixture is too dry and refuses to spread, sprinkle on a
little more turpentine, but do not use too much, else it will take a
long time to evaporate.

The roller having a coat of rather moist ink spread evenly upon it,
place the exposed zinc, face up, on a piece of clean white paper, and
proceed to roll it briskly to and fro, using a moderate amount of
pressure, until the whole of the turpentine has evaporated; it should
leave a thin coat of ink with an even |47| matt surface, not thick
enough to quite hide the yellow film of the sensitive albumen, as, if
it does hide it, too much has been put on, and it will most likely
smear in development.

If, after first applying the roller, the ink on the zinc seems likely
to be too thick, at once wipe the roller dry, and then roll the zinc
briskly until the coat of ink is perfectly even and the turpentine
evaporated.

At this stage everything depends upon getting the coat of ink even.
If there are patches of thick and patches of thin, sprinkle some
turpentine upon the slab, quickly charge the roller, and roll up the
zinc again, until the coat of ink is thin and even.

An even coat of ink being obtained, the zinc is laid in a tray
containing clean cold water of a sufficient depth to well cover the
surface. Now take a pledget of cotton-wool and rub the surface gently,
when the ink covering the albumen protected from light by the black
portions of the negative, will wash away, leaving the picture on the
zinc in ink; if the finer details do not develop easily, continue the
rubbing with the cotton-wool, but be careful not to rub so hard as to
scratch the ink lines.

All details being developed, rinse the picture under the tap and put it
away to dry, which at ordinary temperature will take but a few minutes.

The chances of failure in this portion of the process are, first of
all, air bubbles and dust spots in the film. These will at once declare
themselves. The remedy, is increased care and cleanliness.

If, upon development, some of the lines are missing, then the zinc and
the negative have not been in actual contact, or if the finer lines
wash away easily, then the exposure has not been long enough; whilst if
it has been too long, either the finer details are covered up or the
whole refuses to part with any ink.

A satisfactory print, showing all the lines of the original having been
obtained, dry, by first blotting off the water, then by gentle heat,
after which the zinc is ready for the etching room.

|48|

CHAPTER VI.

PRINTING ON ZINC IN BITUMEN.

The process described in the previous chapter is most suitable for
printing on zinc, for blocks that are not overburthened with fine
lines, and is intended for rough printing; and also, when from want
of sunlight, and the exigencies of business, the exposure has to be
made by electric light; but when the subjects are very fine, and the
blocks must be of the very best, it will be better to print the image
in bitumen; then the first etching can be done without having to ink
up previous to immersing in the acid bath (which must be done after
developing the inked albumen image), so getting the sharpest possible
results, and also securing better depth to close work than when the
inking up has to be done before biting in.

Now the generally accepted idea of bitumen is, that it requires such
a long exposure to light as to be practically useless, except for
direct sun printing; but that only stands good where the bitumen is not
prepared properly and where too thick a film is used upon the plate.

By preparing the bitumen as described below and taking care to have a
very thin film of the sensitive bitumen upon the zinc plate, then the
exposure either to sunlight or electric light is not more than double
that of albumen.

There is one especial virtue in a bitumen film. If by chance too
much exposure to light has been given, a prolonged immersion in the
developing liquid (turpentine) will remedy the defect, whereas if an
albumen image be over-exposed it is quite spoiled, and the work must be
done again.

We are still upon the subject of line work, and the same class of
negative desirable for printing on an albumen film is necessary for
printing upon bitumen, viz., the lines must be clear glass without
veil, and the rest of the negative must be sufficiently opaque to stop
the passage of light.

The sensitive solution of bitumen is made by procuring a small quantity
of photographic bitumen or asphaltum, and powdering it in a clean,
dry mortar. Next take a clean and dry glass beaker, half filled with
methylated ether, and pour into it the powdered bitumen, stirring with
a glass rod for a few minutes; now cover the beaker with a piece of
thin sheet India-rubber, and upon that |49| place a piece of plate
glass, so as to make the vessel as nearly air-tight as possible. Allow
to stand a few hours, then stir up again, and again allow to stand,
this time all night. Then pour away the ether, draining the liquid
as closely as possible, so as to get rid of all those constituents
which are soluble in the ether. Now add some more fresh ether, stir
thoroughly, and again allow to stand and settle, putting on the cover
as before, so as to prevent evaporation. After again settling, the
ether is poured off, and all liquid and semi-liquid matter carefully
drained away. More ether is added, and the operation is repeated
until the added ether, after standing all night, is nearly or quite
colorless. The residue in the beaker is removed to a glass plate and
spread out over its surface, so that any ether remaining may quickly
evaporate. During this evaporation of the ether, the bitumen must be
protected from the action of white light.

By thus purifying with ether we get rid of those constituents of the
bitumen which are not sensitive to light, and thus we secure a film of
bitumen sensitive to the action of light.

When the ether has evaporated, take of the residue half an ounce and
dissolve it in pure benzole (free from water) fifteen ounces, allow it
to stand all night, then filter it through filtering paper (placing a
sheet of glass over the funnel to prevent evaporation). It will keep
six months.

New zinc plates will require polishing first with rotten stone, and
finishing with rouge, but plates that have been used should be first
polished with fine emery cloth, followed by pumice powder, then by
rotten stone, and finished with rouge, remembering that a circular
motion must not be used.

If, after polishing, the surface is at all greasy, immerse it in the
graining bath used for the albumenized plates, wash well and rub away
the scum; then with a perfectly clean piece of blotting paper, remove
the water from the surface and dry it over the spirit flame.

To coat a piece of zinc with bitumen, place it in the whirler, and
when fixed in position, dust the surface with a clean camel’s-hair
brush; then flow over it sufficient of the filtered bitumen solution
in benzole, then lower the whirler and set it in motion; whirl rapidly
for about a minute. This will equalize the coat or film of bitumen
and get rid of superfluous solution. When taken from the whirler the
plate will be ready at once for the printing frame. These plates do not
deteriorate, and a stock of them may be prepared and stored away in the
dark till wanted. Great care must be taken not to allow the slightest
ray of daylight to fall upon them, else the action once set up, will
continue, and spoil the plate. |50|

On examining the zinc plate after removing it from the whirler, it
will be difficult to realize that there is really a sufficient film of
bitumen on the zinc, but there will be quite sufficient.

In printing upon bitumen from negatives that have been varnished, it
will be as well to rub the varnished surface of the negative with a
pledget of cotton dipped in dry French chalk.

The same care in putting into the printing frame, as enjoined in the
chapter on zinc printing with bichromated albumen, is requisite with
these plates, as is also the applying the pressure by means of the
screws. The exposure to light will vary from ten minutes in the sun, to
two or three hours in the shade.

DEVELOPING THE IMAGE.

To develop, place the exposed plate, face up, in a shallow tin tray,
and pour into the tray sufficient turpentine to cover the plate; rock
the tray so as to keep the solution in motion, and (if the exposure
has been right) the image will gradually make its appearance; the
bitumen protected from the action of light by the dense portions of
the negative gradually dissolves away. As the development approaches
completion, great care must be used, and when the last detail is
visible, remove the plate, and rinse it with water from a rose top;
now, if the image is quite perfect, immerse the plate at once in a
mixture of nitric acid and water, the acid being just strong enough to
taste. Keep the tray containing this acid solution rocking for about
a minute, then remove the plate, and wash it thoroughly, rubbing it
very gently with cotton-wool. If the exposure under the negative has
been barely sufficient, the image will be too delicate for touching, so
before rubbing it with the cotton-wool, try some portion of the margin,
and if that stands the friction, it is all right; if not, be content
with rinsing with water.

The immersion in the acid water will have removed the shiny appearance
of the zinc, and the matt surface will enable the operator to see if
all the requisite details of the image are visible. If not, and they
are covered with bitumen, another immersion in the turpentine will
complete the development; but if any of the lines are rotten or the
details are dissolved away, the exposure has been too short, and the
plate will require repolishing and another exposure.

The image being satisfactory, the water is blotted off with clean
blotting paper and allowed to dry. _Don’t use heat for drying._ It may
then be exposed to light for a few minutes. This is not absolutely
necessary, although it tends to make the image finer. The plate is now
ready for etching in relief.

|51|

CHAPTER VII.

DIRECT TRANSFERS TO ZINC.

We have now treated of the various stages necessary to obtain a
photographic transfer upon zinc, from a drawing or engraving, in line,
in dot, or in stipple, first by making therefrom, in the camera, a
negative—same size, reduced, or enlarged—and from that negative a print
on zinc, either in ink on an albumen basis, or in bitumen.

These transfers can be used, either for yielding re-transfers for
lithographic press, or (as is at present our intention) for etching
into relief, for use as blocks for printing from letter-press.

Before proceeding to instruction for etching these photographic
transfers into relief, we will consider the method of dealing with the
direct transfer of drawings, in line or chalk, to zinc, without the
intervention of photography.

For direct transfers to zinc, the picture is drawn by the artist
the exact dimensions of the finished block; if in line, on ordinary
lithographic writing transfer paper, in ordinary lithographic writing
ink, just in the same way that an ordinary line subject is treated for
ordinary lithography.

If the subject is in chalk, it may be drawn on a grained lithographic
stone, which is rolled up, etched, washed out, again rolled up, then
the transfer is pulled; or the picture may be drawn upon specially
prepared transfer paper, like Josz’s polygraphic transfer paper, or
other grained paper made for the purpose; or the subject may already
be on stone, as a lithograph, or it may be a copper-plate engraving,
in which case transfers are pulled and then put down upon zinc in the
ordinary way.

In making drawings on lithographic transfer paper, great care must be
taken to avoid touching the surface with the fingers, as finger-marks
will transfer and roll up black. In line work all lines must be firm
and black; no attempt must be made to get effect by using thin or pale
ink.

In chalk work, also, the drawing must be firm and strong, and the
corrections and alterations made on the transfer, not left to be done
on the stone. If the corrections or alterations are small, they may be
removed with an ink eraser, or by careful washing with turpentine, so
that all the chalk is removed; if the |52| correction be large, paste
a piece of clean transfer paper over the place, spreading the paste as
thin as possible; gum must not be used.

The drawing on transfer paper being obtained, the next step is to
transfer it to stone; then, after rolling up and proving, another
transfer is made, which is to zinc.

From an engraved copper plate a transfer is made on India or upon
Scotch transfer paper, on either a copper-plate press or a lithographic
press, and then transferred direct to the zinc.

The engraved copper plate is first of all examined to see that all the
old ink is out of the lines; if not, wash with turpentine and wipe
quite dry; then, in a piece of clean linen rag, tie up some plate
re-transfer ink; warm the copper plate, either on the hot plate or over
a Bunsen burner, until it can be barely held in the hand; then, holding
it in a piece of cloth to protect the fingers, rub in the ink tied up
in the linen rag, until sufficient is melted to well cover the surface,
taking care to see that the ink is rubbed well into the lines. Then
take a piece of clean, soft rag and wipe off the ink from the surface
of the plate carefully, so as not to remove it from the reversed lines;
this is best secured by wiping across the lines, not with them. When
the surface of the plate is quite free from ink, rub the lower part of
the palm of the hand upon a ball of whiting, and proceed to polish the
surface of the plate. Do not get too much whiting upon the hand, else
it may stick to the ink and prevent it adhering to the transfer paper.

Now place a piece of clean transfer paper (India or Scotch), a little
larger than the plate, face downward upon a piece of clean paper,
sponge the back with a damp sponge, then let it lie a few minutes, so
as to get evenly damp all through.

Now see that the press is ready. If a copper-plate press is to be used,
see that the bed is free from grit, and that the blankets are in place;
if a lithographic press is to be used, put in a stone, wipe it free
from grit, and see that the scraper is all right; remove the tympan if
of leather, but if of zinc or millboard it is all right. Now put the
inked and polished copper plate upon the stone, and the damp transfer
paper, face down, upon the copper plate; then upon the transfer paper
place a piece of printer’s blanket, turn down the tympan, or put a
piece of thin millboard over the blanket, run the bed of the press
under the scraper, turn down the lever, and, if necessary, adjust the
pressure (a good nip is necessary), then run the bed through; now raise
the lever, pull out the bed, lift the tympan and blanket, reverse
the plate, and pull |53| through again. Now gently warm the plate,
and carefully lift away the transfer paper, which should contain the
picture with every line firm and sharp; if it is not so, sufficient
pressure has not been used, or the transfer paper has been made too
damp, or sufficient ink has not been put into the lines.

The transfer, either drawn in line or in chalk, or from a plate, being
obtained, it is next transferred to a polished litho stone. Of course,
the picture can be at once transferred to the zinc which it is intended
to etch, but it will be found best to first of all transfer to stone,
then from the stone pull a transfer, and transfer that to the zinc,
so that in case of an accident during the etching another plate can
be quickly prepared. Before placing them upon the stone, the prepared
transfers should lie in a damping book until evenly damp.

Now take a polished litho stone and place it in front of a fire or
in the sun until it is quite dry, then place it upon the bed of the
press, and adjust the pressure; then place the transfer upon the stone
in such a manner that it lies without any slurring. Next place a piece
of clean paper upon the transfer, then the blanket, lower the tympan,
run in the carriage, lower the lever, and pull through; then lift the
lever, draw back the carriage, turn the stone round and pull through
again, then sponge the back of the transfer with water and pull through
again, repeating the damping, and pulling through three or four times.
Now with a wet sponge saturate the back of the transfer with water, and
lift away the paper, then wash away the composition, leaving the image
on the stone; now cover it with thick gum solution, and allow it to dry.

If more than one transfer is in hand at a time, they are trimmed as
closely as possible and pasted with very thin paste close together
upon a large piece of paper, and then all can be transferred at one
operation.

The gum upon the stone being dry, wash it off carefully with clean
water, then roll up with transfer ink. Clean away any dirt there may
be with sponge and snake stone; where the snake stone cannot be used,
a piece of pointed wood, dipped into acid gum, will clear way the
dirt. Take care to have the wet sponge handy so as to prevent the acid
spreading upon the work; now roll up as strong as possible, then etch,
by passing over water acidulated with nitric acid of such a strength
that it just slightly effervesces when the stone is touched; saturate
a sponge with the weak acidulated water and go gently over the stone,
then with another sponge charged with clean water, wash off the acid.
Now again roll up with transfer ink as strong as possible, and pull
the transfer. Chalk drawings are transferred to stone in the same way,
then etched, but the acid water is allowed to act a little longer than
for a line transfer, and after |54| washing away the etching solution,
the picture is washed out with clean turpentine, then wiped with a
sponge, gummed in, fanned dry, moistened with a wet sponge, and the
water removed. Then the image is rolled up with transfer ink, and the
transfers pulled for subsequent etching.

To transfer to zinc, take a piece of polished zinc and immerse it in
the graining bath (page 40) for about a minute; then remove it, wash
it under the tap, and rub it with soft sponge; then wipe it dry with a
soft rag, and warm the plate slightly; lay it upon a litho stone in the
press, lay the transfer (which has been lying in the damping book) upon
the zinc plate; lay upon the transfer the piece of blanket, lower the
tympan and pull through; then damp the back of the transfer, pull it
through again; then reverse the plate, dampen the back of the transfer,
pull through again; again dampen the back of the transfer, and again
pull through; now saturate the transfer with water, peel off the paper,
remove the composition, and apply with a sponge a sufficiency of a
solution of gum (thickness of cream), 5 ounces; decoction of nutgalls,
10 ounces. The decoction of nutgalls is made as directed on page 56.

Allow this to stay on the zinc for about a minute, then wash off,
cover with plain gum, fan dry, and dip a sponge in gum and rub over
the plate; now dip a soft rag into the gum, then into the etching ink
(page 57) mixed with a little cocoanut oil or mutton fat and middle
varnish, continuing the application of gum and ink until the whole of
the picture is sharp, black, and strong. Be sure and keep the plate
well covered with gum and the ink as thick as possible.

The plate is now dusted with finely powdered resin, sponged with a wet
sponge, and then is placed in the etching trough containing water and
just sufficient nitric acid to taste; in this the plate remains about
half a minute, rocking the etching trough gently all the time; now
remove the plate, wash it under the tap, rubbing gently back and front
with a sponge, then dry by gentle heat; next coat the back, edges, and
margin and portions of the front which are too large to etch away, with
thin shellac varnish. When dry proceed to etch as directed in the next
chapter.

Instead of inking up with the rag after etching with the acid gum, wash
off, then roll up with a leather roller charged with the etching ink
mixed with a little cocoanut oil, and used as stiff as it is possible
to work it, until the image has taken in all possible, damping the zinc
with a sponge directly it shows any signs of getting dry; then dampen
slightly, and repeat as above. Next immerse it in the etching bath as
before; wash well, and dry; coat the back, edges and margin on the
front with shellac varnish, when the plate will be ready for etching.

|55|

CHAPTER VIII.

ETCHING LINE TRANSFERS.

For etching transfers on zinc, whether photographic or direct, we shall
require the following apparatus: A slab of iron about 24 × 18 inches
and 1/2 or 1 inch thick, supported horizontally upon four legs, and
heated by an atmospheric burner, arranged somewhat like a gridiron so
that the heat is even all over. A set of rollers on litho stock, one
of leather, one of flannel, and one or two glazed rollers, the same as
lithographers use for tint printing—we also require an etching box—_i.
e._, a wooden tray, 30 × 24 inches, and 8 inches deep, well made of
seasoned wood, lined with either pitch (with a little tallow added), or
gutta-percha, and mounted upon rockers.

This box will require a firm table for its support during the etching,
said table standing as close as convenient to a sink and water tap.

The other requisites used during etching, are, nitric acid, turpentine,
gum Arabic of a good quality, some powdered nutgalls, three or four
sponges, some finely powdered resin, a flat camel’s-hair brush, a
solution of shellac in spirits of wine, and the following inks:

First the etching ink, composed of beeswax one-quarter ounce, Russian
tallow two ounces, bitumen half an ounce, middle varnish two ounces.

Melt these together in a pan over a fire, or Bunsen burner, stirring
well during the operation, so as to mix them thoroughly; when all are
melted, add five ounces of ordinary letterpress printing-ink, and
thoroughly mix; then allow to boil and continue the heat until the gas
escaping from the bursting bubbles explodes upon the application of a
lighted taper; then remove all from the fire, and allow to cool.

For a hard ink, for use after the plate is etched deep enough, and the
resist is cleaned off, mix

Beeswax 1/2 ounce.
Resin 1 ounce.
Shoemaker’s Wax 1 ounce.
Black Litho Ink (about $1 a pound) 2 ounces. |56|

Melt, then cool and mix with turpentine to make it the consistency of
soft soap.

Now, with these and a solution of gum Arabic (in cold water), the
thickness of cream, add one-quarter pint of a decoction of nutgalls to
each quart of gum solution. The decoction of nutgalls is made by adding
one-quarter pound of bruised nutgalls to one and one-half pints of
water, in an earthenware vessel (not metal); boil, then allow to stand
at the fire and simmer gently for six hours, keeping the vessel covered
over; then allow to cool, filter and add the proper quantity to the
above gum solution.

We will assume that a suitable place is provided for carrying on the
operations to be described, in the shape of plenty of bench room, and a
good light to work by.

The first stage in etching a zinc plate in relief is, to slightly warm
it upon the hot plate, then allow it to cool (by-the-bye, it will be
very convenient to have a clean litho stone handy for placing the plate
upon to cool quickly). The plate being cold, with a piece of soft
sponge carefully smear it over with the gum solution, allow the gum to
dry, spontaneously, in a cold current of air; if heat be applied the
gum will crack and bring away the image from the plate.

Whilst the gum is drying, with a palette knife place equal parts of
transfer ink (page 44) and of etching ink (page 54) upon one corner of
the inking slab, then thin to the consistency of cream, with middle
varnish, thoroughly incorporating the three ingredients with the
palette knife.

Now place a little of this ink upon the leather roller and roll
vigorously upon the slab, so as to distribute the ink thoroughly upon
both roller and slab; be careful not to get too much ink on the roller,
nor to have it too thin; in fact, work the ink as stiff as is possible.

Now lay the zinc upon a piece of clean paper, and sponge it gently over
with a wet sponge, so as to loosen the film of gum, then squeeze the
sponge nearly dry, and pass it over the plate again, so as to insure it
being evenly damp all over, but be careful not to make it too dry.

Now proceed to roll up, by passing the charged roller to and fro over
the plate, using moderate pressure and slow motion, recharging the
roller at short intervals from the inking slab. Occasionally use the
damp sponge so as to keep the plate sufficiently damp to resist the ink.

If the roller slides instead of rolling, wipe it with an old linen rag,
which will remove the moisture; then recharge the roller again upon the
slab. |57|

The rolling is continued until the whole image is an intense black,
when it is carefully dusted over with very finely powdered resin
applied with a broad camel’s-hair brush, taking care that all the image
gets covered. Then rub it gently with a wet, soft sponge and place it
in the etching box containing a mixture of water and nitric acid, the
acid being only just perceptible to the taste.

The plate should remain in this for one minute (the box being kept
rocking); it is then removed, and thoroughly washed back and front
under the tap. Rub it gently with a clean soft sponge.

This etching is merely to remove any traces of gum or dirt from the
zinc which would interfere with the shellac varnish holding.

Now dry the plates, using gentle heat, then coat the back with thin
shellac varnish to protect it from the acid; do the same to the margin
of the picture on front, also varnish the centre of any very broad
whites up to half an inch of the image, so that the acid dissolves no
more zinc than is necessary. Now examine the image carefully, and if
any of the lines are defective touch them up, and make any alterations
and additions required.

The plate is now ready for the first etching, for which purpose a
little nitric acid is added to the water in the etching tray—precise
directions cannot be given as to how much acid to add, as so much
depends upon the area of zinc on the plate that requires dissolving;
practice, however, will soon enable the operator to judge the proper
quantity. If too much acid is added, the plate will quickly be covered
with myriads of minute bubbles, in which case it must be instantly
removed, well washed, and the bath diluted with water before the plate
is reimmersed. If, on the other hand, there is too little acid present,
the action is too slow, and more must be added.

The first etching must be carefully watched, and the rocking continued,
until the application of the finger-nail to the margin shows that the
zinc inside has been dissolved away to a depth of about the thickness
of a visiting card.

The first etching is the most important of the whole, as unless a
sufficient depth be attained the sharp lines will not be obtained; and
as the ink is not yet capable of resisting too strong acid, great care
must be taken that the work is not damaged; proceed cautiously, adding
acid from time to time as required.

As a rule, the first etching will take from five to ten minutes (the
tray being kept rocking all the time).

When it is judged that the first etching has been carried far enough,
remove the plate from the tray, wash it well under the tap, rubbing
gently with a |58| sponge, so as to remove the scum left by the acid,
dry by means of gentle heat, then allow it to cool.

When the plate is quite cold, smear it over with gum solution, and with
a piece of cardboard, fan the gum dry.

Now sprinkle the inking slab with turpentine, and with a cloth wipe
the slab clean. Take a piece of etching ink and thin it with middle
varnish, mixing them well with the palette knife upon the slab; now
take the leather roller, and with the palette knife place a little of
the ink upon it, and roll up on the slab until both roller and slab are
well coated; but on no account must there be too much ink, nor must it
be too thin.

Now lay the zinc down on the bench, on a piece of clean paper, and with
the wet sponge carefully wash off the gum; then wipe all superfluous
water off the plate, and roll up with the leather roller charged as
above; roll the plate first one way, and then the other, keeping the
zinc evenly damp all over, else the ink will catch in the whites, and
probably spoil the picture. When the rolling is completed, and as much
ink as possible has been piled on, the zinc will be nearly dry. If not,
allow it to stand in a cold current for a little time, then take it to
the drawer in which the powdered resin is kept, and smear the plate
all over with the powder. Now brush as much of the resin away as will
come, using the brush from all sides, so that all the lines get evenly
coated, not only on the top, but upon the sides; this being done, take
a damp sponge and carefully remove the superfluous resin from the
whites, or unprotected zinc.

The plate is now ready for the second etching, and the solution in
the etching tray must be reinforced by the addition of a little acid;
but do not add too much at once. It will be far best to add a little
at a time, and then, as soon as the zinc shows there is no action
going on, add a little more; an easy and simple method of ascertaining
whether any acid be present or not is to wipe the bare metal with the
tip of the finger, and if that spot (which will be brighter than the
surrounding parts) does not speedily resume its dingy color, the acid
is exhausted.

The plate being immersed in the solution, set the tray rocking, and pay
attention to the remarks above. At the end of ten minutes remove the
plate from the tray, wash it under the tap, rub it gently with soft
sponge, then remove as much of the water as possible, and examine the
progress made by the acid. This can be seen by the lines being bare
below the ink, in which case the etching has been carried far enough,
and if not stopped, there would be danger |59| of under-cutting; if,
however, no progress has been made, add a little more acid to the
solution, replace the zinc, and rock again for another five or ten
minutes.

The second etching being effected, the zinc is carefully washed, and
the scum left by the acid is carefully sponged away; now stand the zinc
up near the hot plate, so that it will get the benefit of a gentle
heat, and when quite dry lay it upon the hot plate (which should be
heated to a temperature of 120° to 150° F.) face up, with a piece of
brown paper between the zinc plate and the hot plate.

As soon as the zinc plate begins to get hot, there will be a tendency
to curl slightly away from the hot plate, which, if allowed, would
prevent the ink being evenly melted. To prevent this, take a brad-awl
in each hand, and press down the sides of the zinc, taking care not to
touch any of the picture.

Allow the zinc to remain on the hot plate until the ink and resin are
melted and run down to the bottom of the etching, then remove it and
lay it on the cold slab until the plate is cold.

When cold, smear the plate with the gum solution, fan it dry (_never
use heat for drying the gum_), moisten with wet sponge, roll up again
(use the leather roller), using the ink pretty stiff on the inking
slab; keep the surface of the zinc well moistened. When the roller gets
too much water upon it, pass a piece of damp cheese-cloth over it to
remove the water; then roll the roller vigorously on the slab until it
again bites the ink. Continue rolling the zinc until all portions have
received due attention from the roller. N. B.—Some of the closest work
will be quite blocked up this time, and each subsequent rolling will
block up more and more, until only the very open work will be left.

Now allow the zinc to get dry, then cover it with resin, brushing from
all sides, so as to coat the sides of the lines as well as the top, and
then remove all superfluous resin from the whites with a damp sponge.
The zinc is now ready for the next etching, for which more acid is
added to the solution in the etching tray.

Rock the tray carefully, watching the zinc to see that the acid is
neither too weak nor too strong, until the progress can be seen by
examining the plate; the time, with the proper quantity of acid, is
twenty to thirty minutes.

When the etching has proceeded far enough, after washing and sponging,
again allow it to dry, then place it upon the hot plate until the ink
is melted and runs down the sides of the lines; then cool, smear with
gum, fan dry, moisten with sponge, and roll up as before; dry, cover
with resin, using a |60| camel’s-hair brush, then dampen with a sponge
and give a fourth etching, using the same precautions as to strength of
acid and duration of rocking as before.

Now cool the plate; get a little more ink on the roller, and roll the
plate whilst cold. When the surface of the lines has a nice even coat
of ink upon each and all (coarse and fine), again warm the zinc on the
hot plate until it is just too hot to hold in the fingers; then cool
it again, varnish the back with shellac varnish, then make a mark with
a blunt point, in the ink on the margin, so as to lay a short line of
zinc bare to the action of the acid.

The round of operations is repeated; but for rolling up for the fifth
and subsequent etching, a flannel roller is used, and more ink will be
required upon the slab; it will also require to be a little thinner.

For some subjects six or seven etchings will be required, whilst for
others—especially where there are whites that are too small for cutting
out with a fret saw or router—ten or twelve etches will be required.
Practice, the best teacher, will soon enable the operator to judge how
many are required.

The etching having been carried as deep as is judged sufficient,
sprinkle the plate liberally with turpentine, and with a stiff
scrubbing brush loosen the ink from the lines, and wash it off with a
solution of American potash.

The plate being cleared from all ink, etc., is now examined carefully.
The sides of the lines will show each etching, by a series of irregular
steps. If the plate be put into the press in this condition, the
chances are that before many copies had been made, these steps would
take more or less ink from the rollers, and blur the image; therefore,
before passing it into the hands of the printer, the plate will require
etching two or three times more, to get rid of these irregularities.

This is done by warming the zinc on the hot plate, and then, whilst
still warm, rolling up with a fine glazed roller charged with the hard
etching ink from a clean inking slab.

Roll the zinc firmly, first one way and then the other, so that all
the tops of the lines get well coated with ink; now make a mark on the
margin with a blunt point in the ink, so as to lay a short line of zinc
bare to the action of the acid.

Next empty the etching tray, put into it some clean water, and add
sufficient acid to make it taste like strong vinegar; in this immerse
the plate, and keep rocking for ten or fifteen minutes, or until the
mark on the margin, when felt with the finger-nail, shows that it has
attained a depth about the same as that obtained in the first etching.
|61|

Now wash the plate under the tap, and wash off the ink with turpentine,
followed by a solution of American potash; again wash and dry on the
hot plate. Now examine, and if the lines are free from the steps, the
plate is finished, but if not, the operation must be repeated until the
steps are all removed.

Be careful to cover the surface of the block thoroughly with the ink,
else the acid will spoil the picture.

The plate is now ready either for mounting for the press, or for
electrotypes being taken from it; if the former, the deep whites
are cut away with the router or fret saw, the edges are trimmed or
bevelled, holes are drilled and counter-sunk at convenient places, for
the insertion of nails or screws to fix the zinc to the wooden block,
to make the surface type high.

The object aimed at in the instruction in Part I. is the production
of relief blocks on zinc from an original in black and white, which
original may be a drawing made purposely for reproduction, or it may
be from a drawing already in existence, a woodcut, or engraving,
the picture being rendered entirely in line, or a chalk drawing may
be used. In fact, any subject that is capable of being worked from
either at a type press or by ordinary (monochrome) lithography. Washed
drawings, or oil or water color drawings are not applicable.

In fixing plans, or drawings on the easel, prior to photographing them,
if they are cockled, and difficult to get flat, pins may be placed
anywhere, so long as the lines are not interfered with, for these pins
may be painted out with a camel’s-hair brush and gamboge or Indian ink.
It is important that the plans or drawings be as flat as possible, as
if the lines are cockled, they will not be photographed straight.

In photographing drawings on tracing paper or cloth, a piece of white
paper should be placed behind them.

When, from an original of black lines on a white ground, it is desired
to make a reverse block—_i. e._, white lines on a black ground—a
negative is first made from the original, and from that negative
a transparency is made; and a print made upon the zinc from that
transparency will be a reverse of the original.

Thus far I have tried to make plain the details of a process which is
as fascinating and as pretty as any in photography, and which supplies
results which could not be attained by the most expert workers two
years ago. And since those experts first obtained even tolerable
results by zinc etching, like |62| everything else in photography,
it has made wonderful progress. At first we were delighted and
content when a block was obtained with relief sufficient to enable
us to print it upon an ordinary press with type. But now we can
get from the zinc surface all the qualities which are given by the
lithographic stone. Indeed, the process of zincography bears a very
strong general resemblance to that of lithography; of course, it
varies therefrom in matters of process detail. The manipulations of
zincography, however, are no more complicated in their nature than the
details of printing, etc., from stone. Crayon drawings, ink work in
line and stipple, rubber work, in fact, anything that can be drawn on
stone can be drawn on properly prepared zinc, with the exception of
engraved lines (intaglio), the structure of the zinc not giving the
yielding brittleness of stone. The great departure made possible by
zinc plates exists in the fact that they can be bent to the surface of
a cylinder, thus displacing the reciprocating bed and stop-cylinder
of the lithographic press with the continuously rotating plate and
impression cylinder of the zincographic press, which, at the same
driving speed, produces double the number of impressions printed on
the lithographic press. To Mr. Bernard Huber, of the Huber Printing
Press Company of Taunton, Mass., belongs the credit of designing the
only American zincographic press in existence, and which is now in
successful operation in several lithographic establishments. It is a
thoroughly American machine in design and construction, and while no
glowing prophecies of its immediately taking the place of lithographic
presses are indulged in, yet this kind of press has its place and use,
and will by its qualities win favor in the trade.

Many lithographers are beginning to give correct attention to
zincography, but few are willing to give the time and constant
experimenting to the subject that has been given by Messrs. Harris &
Jones, who during the past three years have operated the zincographic
presses in their lithographic establishment known as the Providence
Lithograph Co. Having taken the selling agency of the Huber
zincographic press, they offer to those who _buy_ the press full
instructions in zincographic surface printing.

These suggestions are given right here, first because we are now about
to take a step higher in zinc etching—a step which will lead us to
results which lithography can scarcely equal in some particulars—and
second, because it is the policy of this work to withhold no
information which the novice will need in supplying himself with a
perfect outfit for doing the best of work. For the same reason the
advertisers have been chosen, rather than received in the usual way.

|63|

PART II.

PHOTO-ENGRAVING IN HALF-TONE.

CHAPTER I.

RETROSPECTIVE.

The former chapters have treated entirely upon the production of blocks
in line—_i. e._, where the picture has been made by a draughtsman,
the half-tones and gradations being communicated by a greater or less
thickness of line, or by dots, or stipple, or hatching.

The picture for such blocks may have been specially drawn for the
process, the same size or larger, or it may be a copy of some woodcut
or engraving already in existence, but if it is desired to reproduce
blocks from drawings, paintings, or photographs, then an entirely
different method must be adopted, and the smooth gradations of
half-tone levelled, so to speak, so as to bring the high lights and the
shadows upon one plane.

In photographs from nature (or from washed drawings or paintings) the
scale of gradations runs, as it were, in a series of short steps from
the deepest shadow to the highest light, and a block made, say in
bichromated gelatine, from such a negative can give no half-tones, as
the inking roller could only touch the deep shadows properly.

Now the subject of making photographs applicable for the illustration
of letter-press, instead of woodcuts, has occupied the attention of
experimentalists from the early days of the art-science, as the records
of the Patent Office show.

The first patent, dated 1852, bears the honored name of Mr. Fox Talbot,
and although it is for intaglio printing, and therefore a little out of
place under the above heading, still it claims our attention as giving
a method for breaking up the half-tones of the photograph, by placing
muslin, crape, etc., between the photographic cliche and the sensitive
surface; or a glass plate may be covered with fine lines, or glass may
be coated with powder, which is caused to adhere. |64|

In 1854, Paul Pretsch broke up the half-tone by the reticulation of
gelatine, caused by the admixture with iodide of silver and bichromate
of potash; this was spread upon a silvered copper plate, dried, and
exposed to light under the half-tone negative, then washed in cold
water and borax, or carbonate of soda, then in alcohol, coated with
copal varnish, and immersed in a weak solution of tannin, after which
an electrotype could be made, or a transfer made to zinc or stone.

In 1855, A. J. Berchtold produced a grain by printing upon a photograph
in black or in any color, from a plate or block or other surface, or
by perforating or making strokes, lines, or dots upon it, by roller or
other instrument. Repatented in 1883, by Brown, Barnes, and Bell.

In 1860, E. J. Asser used starch, and in 1865, J. W. Swan used a tissue
of gelatine mixed with charcoal or other chemically inert grit; in
the same year Messrs. E. & J. Bullock published, perhaps, the most
important specification, describing all, or nearly all, practical
methods of obtaining grain, the most important of which are the
placing of any fine fabric between the lens and the sensitive surface,
or between the camera and the object, or copies of granulated or
recticulated structures or fabrics could be used, or such copy could be
placed in contact with negatives, and both copied together.

In 1879, J. W. Swan made negatives by moving, during exposure, the
Bullock’s screen, placed in front of a sensitive plate. Meisenbach’s
method, patented a little later, is somewhat similar.

If a Woodbury relief is thinly coated with transfer ink, and then laid
upon a piece of ordinary litho transfer paper which has been embossed
with lines, or dots, or stipple, by being pressed in contact with wire
gauze or an engraved plate, and the inked relief and the embossed litho
transfer are then subjected to heavy pressure, a grained image is
impressed upon the transfer paper, which can be transferred to zinc,
and then etched in relief.

The method of making a grained negative to be now described, shortly
stated, is done by interposing a screen, either before the sensitive
plate in the dark slide of the camera (when copying a photograph) or
placing the screen behind a transparency on glass when transmitted
light is used. In the first instance the image projected upon the
sensitive plate, having first to pass through the screen, is broken
up by the dots upon the screen, the result being a definite grained
negative. In the second instance, the screen being placed in contact
with the transparency, a similar result follows. The first method
is most generally used, as the print does not require the careful
focussing necessitated by the second.

|65|

CHAPTER II.

MAKING GRAINED NEGATIVES.

THE SCREEN.

For making grained negatives, the apparatus, chemicals, and
manipulations described in Chapters I. and II., Part I., for line
negatives, are required, with perhaps a little increased care to secure
clean and bright negatives.

The first requirement will be a proof, on fine white paper, from a
machine-ruled plate, or a plate with fine dots or stipple; a favorite
being plates ruled diagonally and straight, either in single lines or
crossed. These plates must be of good size, say 18 by 15, ruled with
lines as fine as possible, 100 or 150 to the inch. The ruled sheet must
be perfect, as any defect in it will be fatal.

Such a proof being secured, it should be carefully mounted with starch
paste upon a stout piece of smooth cardboard, and should be carefully
shielded from all chances of being soiled, as the slightest stain
or mark upon it will unfit it for use. As such a fine line is very
difficult to focus, especially in making the smaller screens, it will
be found a good plan to cut four narrow strips of good, bold type, and
paste these at the four corners of the sheet, just outside the ruling;
these slips of type will be easy to focus, and will render the task of
making the screens easier.

Plates ruled with single lines, either diagonally or horizontally, may
be used instead of the cross ruling, and are by many preferred.

Those in possession of a ruling machine may make these ruled sheets by
ruling a large litho stone, and pulling impressions from that stone.
If this is done once, and done well, the sheets will last a lifetime;
and if the stone be sufficiently large, and the lines very fine, the
screens may be used for blocks 15 by 12 inches or larger.

To copy this ruled sheet, remove the mirror from the lens, and put the
lens in the camera in its ordinary position; then pin up the sheet
on the easel, and, after seeing that the easel and camera are quite
parallel, proceed to make a series of negatives from the sheet, making
screens of various degrees of fineness, varying from a coarse grain for
a coarse photograph, to the finest possible for |66| photographs full
of delicate half-tone, and from three inches to ten inches wide. Many
subjects will need screens made especially for them. The screens must
be free from speck or stain, and should be made upon very thin glass.

The nitrate bath should be in good condition, and the collodion ripe.
Such negatives take a good deal of time making, but as they are the
foundation of the process, and with care will last for years, the
trouble must not be grudged.

The screen negatives being made, they must be varnished with a good,
hard, well-filtered varnish, applied in a room quite free from dust.

The screens must be made by the wet collodion process. The ordinary
gelatine dry-plate is utterly useless for such work. Gelatino-chloride
plates might do, but the exposure is so very long that there is risk of
shaking the camera during exposure.

THE GRAINED NEGATIVE.

For the first method a good vigorous photograph is selected, placed in
position on a copying board, and the camera adjusted so as to get the
image on the focussing screen the size wanted the mirror being used, as
the negative must be reversed.

A collodion plate is now prepared and well drained; then one of the
transparent screens is fixed in front of the carrier by drawing pins,
by passing strips of gum paper over, or by fixing with fine tacks
a piece of thin card at the top, and one at the bottom, slightly
overlapping the screen, and holding it firmly in a sort of rebate.

The carrier is now placed in the dark slide, the sensitive plate in its
place, the door of the slide closed and fastened.

The exposure is now made in the camera, and if the screen is properly
transparent the time will not be very much more than when copying in
the ordinary way.

The development of the exposed plate is done by means of the developer
given in Chapter I., and the result must have all the details of the
photograph, while the lines of the screen must be clear and free from
veil.

The negative is washed, fixed in cyanide, washed again and then
intensified, first immersing it in the solution No. 1, Chapter I.,
until bleached, then thoroughly washed and blacked with No. 2 solution,
again washed, and varnished with the water varnish, or dried and
varnished with benzole varnish.

For the second method we shall require, instead of a paper photograph,
a transparency on glass. |67|

The transparency may be made on a gelatine dry-plate by printing in
contact with the negative, or an enlarged transparency may be made,
either on a dry plate or by the wet collodion process.

The transparency should be made by contact, when the original negative
is of larger size than the block required; the enlarged transparency is
used if the negative be smaller or the same size as the block.

The development of the transparencies on gelatine dry-plates will be
treated of later, but if wet collodion be used, the manipulations will
be the same as for negatives, except that the image is in reverse
gradations, the lights being clear glass, and the shades dense and
black. Every detail in lights, shadows, and half-tones must show
distinct and strong.

[Illustration: Fig. 5.]

For the production of these enlarged transparencies, an enlarging
camera will be required, which may be provided by having an arrangement
in front of the ordinary camera, fitted like the accompanying figure,
consisting of two boxes, one sliding within the other, the negative
from which the transparency is to be made being placed in a carrier at
B.

In the illustration the sides are shown open, but only for simplicity,
as they must be quite opaque. In using such an arrangement, the camera
must be brought under the skylight of the studio, and the light
reflected through the negative, by placing a large sheet of white paper
at an angle of forty-five degrees in front of the negative.

Another and perhaps better method will be to cut a hole in a dark-room
at a proper height for the camera, and fix the negative in the hole,
then adjust the focus upon the screen, illuminating the negative by
means of a reflector fixed at an angle of forty-five degrees.

The transparency being secured, it is varnished, and all blemishes or
spots removed by means of a sable brush, and a little carmine color; it
is then placed in contact with a suitable screen, and the two together
are inserted in the |68| place previously occupied by the original
negative. Now adjust the camera so as to get the image on the focussing
screen the proper size, and proceed to make a grained negative by the
wet collodion process exactly as described in Chapter II., Part I.,
and above. When a negative containing all the details of the original
negative broken up by the fine grain of the screen is obtained, it may
be dried and varnished, and then it is ready for printing upon the zinc.

All pinholes, etc., should be stopped by means of a fine sable brush
and Indian ink. The printing on the zinc should be done by the bitumen
process, Chapter VI., Part I., as the albumen is not nearly so perfect.
If, however, the albumen process be preferred, the printing is done in
the same way as described in Chapter V., but extra care must be taken,
first, that the zinc plate is thoroughly and evenly polished; secondly,
that the graining bath is kept weak with plenty of alum in, so as to
have the grain on the plate as fine as possible; thirdly, that no
speck of dust, dirt, or any air-bubbles be on the film after coating,
and that the whirling be effectually done so as to get the sensitive
coating as even as possible.

The inking up requires no comment, as it must be done as evenly and
thinly as possible, for both line and half-tone.

In development, a little more energetic friction will be necessary, but
extreme care must be taken not to abrade the ink surface. Continue the
rubbing until all the details are developed, and bear in mind that the
finished block will be exactly like the zinc after development.

In printing these half-tone zincs, it often happens (like printing
in silver) that to get the best results some portions will require
less exposure than others. The best way to stop back any portion or
portions, is to cover the front glass of the printing frame with
whiting mixed with water to the consistency of thick cream; apply with
a rag over the places in the negative, before exposing to light, and
at the end of one-third, or in case of very deep shades, one-half the
exposure, clean off the whiting and finish the exposure without any
obstruction to the light.

The exposure to a grained half-tone negative will be one-half to double
as long as a simple line negative.

A perfect print on the zinc must contain all the grain intact, for
if there is any break in its continuity, it is of no use to proceed
further with it.

The printing in bitumen requires no more comment than to say care is
necessary to avoid dust. The smallest speck will be likely to spoil an
otherwise perfect print.

|69|

CHAPTER III.

ETCHING IN HALF-TONE.

WHEN THE PRINT IS IN ALBUMEN.

The zinc plate with the image upon it in ink, is dried, then warmed
slightly on the hot plate, cooled, and coated with thick gum* and
fanned dry (not dried by heat, or the gum is certain to crack and bring
away the image or part of it); then wash it under the tap, and rub it
gently with a fine sponge so as to remove all gum from the ink, but
not from the zinc. Next proceed to roll up as directed in Chapter V.,
using the India-rubber roller charged with stiff ink. The surface of
the zinc should be kept well covered with water. Use as little pressure
as possible, but let the motion be fairly rapid, and if any portions of
the image should smear, roll rapidly with slightly increased pressure.

* See page 55, Part I., Gum and Nut-galls.

This operation of rolling up the image is the crucial one, for unless
it is done properly, when it is finished, the result is a strong black
and perfectly even image; it is of no use proceeding further with it,
for in fact the picture must be perfect.

The rolling up being done, any touching up that may be required can
now be done, and any fine details clouded over, or made indistinct by
the grain, strengthened or opened out. Additions should be made with
transfer ink thinned with turpentine, laid on with a very fine sable
brush. The whites are put in by scratching through the ink with a fine
etching needle.

To rest the hand upon in doing this touching up, so as to avoid
touching the image, a bridge is used made of a strip of smooth wood,
one inch wide, quarter of an inch thick, and sufficiently long to well
span the plate; at each end of this strip nail narrow strips a quarter
of an inch thick to serve as the feet for the bridge to stand upon.
Then the zinc may be slid under it without touching the surface against
the under part of the bridge.

The zinc is now ready for the first etching in the rocking tray.
The nitric acid solution must be very weak indeed to the taste, the
presence of acid being just perceptible. The time of immersion in the
first bath must not be longer |70| than thirty seconds; then the zinc
is removed, washed under the tap, and gently rubbed with a sponge; dry
it gently on the hot plate, allow the zinc to cool, coat it with gum,
fan it dry, rinse it under the tap and rub it with a sponge; then again
roll up, when it is ready for the second etching; that is done in the
same bath as the first, without any addition of acid. Keep the tray
gently rocking for three minutes, then again withdraw, wash it under
the tap, rubbing with sponge, coat with gum, fan dry, wash under the
tap rubbing gently with sponge, and again roll up, using the ink on
the roller a little thicker, but stiff. When the image has taken the
ink equally, place it on the hot plate and allow the zinc to get hot
enough to melt the ink slightly; then allow it to cool, and place it in
the etching bath, slightly reinforced with a few drops of nitric acid.
Immerse it this time for five minutes.

The operations of washing, gumming, rolling up, etc., are to be
repeated until it is judged that the etching has been carried far
enough. The time of immersion in the acid solution with each etching
may be lengthened, but take special care to keep the bath weak until
near the last etching, when the strength may be slightly increased.

The resist is cleaned off with turpentine and a stiff brush, and then a
proof is pulled. If further etching will improve it wholly or in part,
the plate is inked up and again subjected to the action of the acid
bath.

If only portions require reëtching, cover the rest with bitumen
varnish; but it will be scarcely safe to give more than one etching
after cleaning off the original resist.

WHEN THE IMAGE IS IN BITUMEN.

A bitumen image is etched in the first bath in which the acid is
just perceptible to the taste, without any preliminary rolling up.
The duration of the first etching may be prolonged for three or five
minutes; then the plate is withdrawn and well washed. Remove any scum
with a soft sponge; then dry it in a cold current, and smear it with
gum, fan it dry, and roll up with a leather roller charged with stiff
ink, until all portions of the image have taken a film of ink. Now
reinforce the nitrate bath with a few drops of nitric acid, and again
immerse the plate, rocking the bath for ten minutes; watch the picture
carefully so that in case of undercutting the plate may be removed
before any mischief is done.

The plate is again removed, washed, rubbed with a sponge, and dried; it
is |71| then warmed on the hot plate, so as to slightly melt the ink,
then allowed to cool, smeared with gum, fanned dry, damped over with
a wet sponge, and rolled up, the roller being charged with stiff ink.
The plate is now ready for another etching, for which the bath must
be strengthened by the addition of more acid. The immersion (rocking
all the time) may be fifteen or twenty minutes, after which the plate
is withdrawn, washed, rubbed with a sponge, and if it is thought
another etching would improve it, the cycle of operations is repeated,
beginning with warming the zinc on the hot plate.

After the resist is cleaned off (which with bitumen must be done first
with turpentine and then with benzoline) further etching may be given,
if deemed necessary, first inking up well with the hard ink mentioned
in Chapter VIII., and then reimmersing in a weak bath of acid and
water. If only a portion requires reëtching, those parts that are not
to be touched, are protected by coating with bitumen varnish.

The plate being etched, now requires finishing.

The outside zinc is removed with a circular saw and then the edges are
filed and holes drilled at an angle, so that the metal can be fixed
upon the block.

|72|

CHAPTER IV.

PRINTING FROM THE BLOCK.

A half-tone block to give results commensurate with the care needed
in its preparation, must be handled by the machine man with care and
consideration.

The blanket on the tympan or cylinder must be replaced with something
harder, else the soft pressure of the blanket will blur the print.

The block must also be made ready, not by putting cut-outs on the
tympan or cylinder, but underneath the block, and there as thin as
possible.

The ink must be good and not too thin; the rollers must be free from
flaws and not too tacky. In fact, as much care is required on the
press as during the photographic and subsequent operations. Indeed
photo-engraving and zinc etching would have come into popular use
more rapidly than they have, if printers had been willing to give
them the special “making-ready” attention they require. Despite all
prejudice and indifference, “process-engraving” so called, has made
continuous improvement ever since it came into use, and the good work
goes on. The most delicate gradations of light and shade discernible
in nature, may, from the photographic plate, be rendered in pure black
and white by means of any of the methods given in this work. All that
nature displays, and all that imagination compels, may be reproduced
indefinitely.

With regard to the storage and keeping of zinc blocks after using, Mr.
T. Bolas, in the _Photographic News_ of September 24, 1886, says, “they
should not be washed with the usual lye, but should have a few drops
of paraffine oil poured upon them; and after this has been well rubbed
in by a soft brush kept for the purpose, the paraffine should be well
wiped away with a soft cloth. If the block is to be stored away for a
long time, it should be waxed. The best way of doing this will be to
make it rather warmer than is necessary to melt wax, and then to rub it
over with a piece of yellow bees’-wax, after which the excess is wiped
off with a piece of flannel.”

Sometimes zinc blocks are electroplated with copper or nickel (a
necessity when they are to be used for certain color work), and such
blocks should also be treated in the same way as the bare zinc, as they
cannot be safely cleaned with the lye solution.

|73|

CHAPTER V.

THE TRANSFER OF THE DRAWING, AND ITS TREATMENT BEFORE ETCHING.

According to the methods of producing them, classify the drawings as
follows:

(_a_) Freehand drawings in crayon or ink, drawn with lithographical
chalk on rough paper, or with pen and chemical Indian ink on paper
prepared for transferring.

(_b_) Lithographical transfer of engravings, pen-and-ink crayon
drawings, or drawings on stone.

(_c_) Transfers from relief plates made in copper, steel, zinc, or lead
(music).

(_d_) Anastatic transfers.

(_e_) Fat or resin prints from photographic negatives.

Proceed as follows:

(_a_) _Transfer of hand-drawing._—Place the drawing to be transferred
with its face upon a sheet of clean, white paper, and moisten the
back with a weak solution of nitric acid (1/2° Baumé), by means of a
sponge. Over-moistening causes obliteration of the drawing, fringing
of the single lines, and the running together of the hatched portions.
The correct degree of moisture can be ascertained when the side
prepared and drawn upon grows slightly sticky, and when the drawing
becomes glossy. This will take place in from four to five minutes
after moistening. This time is to be spent in arranging the zinc in
the press, after having freed it from all greasiness. Place a card on
the rolling press below the drawing and the zinc; above it, a sheet
of good blotting-paper, a sheet of Bristol paper and are of pressing
board; then make a trial print with the press, a clean piece of paper
taking the place of the drawing. The correct pressure is a matter of
experience; it is advisable to begin with a pressure less by one sheet,
in order to be able to increase it during the process of transfer.

In the lithographic press the ink-block is first to be adjusted; since
it needs a greater “setting in” than the rolling press, the zinc must
be cut larger. It must extend three centimetres on all sides beyond
the drawing. The edges of the cut plate must be well ground off, in
order that the ink-block may not be |74| caught; at all events, it is
advisable to have the latter smaller than the plate. Observe that the
range of the press should be regulated; then place the zinc directly,
without any intervening layer of paper, on a solid stone; lay upon it
a clean sheet of paper, a blotter, a sheet of Bristol paper, and a
pressing board well covered with tallow. Make a trial by drawing the
sheet through at a moderate pressure. If all is arranged, the work of
transfer can be started. The temperature of the zinc should now be
about 35° C.

Place the drawing down carefully, without moving it about; upon it the
blotter, the Bristol paper, and a pressing board, and draw it through
three times with constantly increasing pressure; turn the plate in
a contrary direction, and draw it through three times in the same
manner. Now place a moistened sheet of good paper between the blotter
and the drawing, and draw through, first with weak, and then with
strong pressure, three times in both positions. Instead of turning the
zinc, the ink-block may be reversed. This finishes the operation of
transprinting, and the next question is the loosening of the paper from
the zinc. Here we can pursue two methods: first, we can have hot water
and a porcelain tray at hand; place the copied plate in the tray, and
pour the water upon it. The coated layer bearing the drawing begins to
separate from the paper. Shaking the tray promotes this action, and
soon the paper will loosen itself from the layer which remains attached
to the zinc. With the second method proceed thus: moisten the back of
the copied drawing, thoroughly with a sponge and cold water; allow it
to soak in, warm the plate to 60°–65° C. and carefully rub all parts by
hand. The layer will again separate by degrees from the paper, which
latter we can then easily lift off from the plate.

On account of the strongly gelatinous layer, crayons on grained paper
should only be moistened moderately before and after the first rolling,
in order to avoid the coiling of the paper.

Hand-drawings on paper without coloring require treatment with stronger
acid (I recommend nitric acid, 4° Beaumé). At the same time the drawing
should be cut as close as possible. To draw it through securely, place
it as usual upon the zinc, and above it a piece of prepared copy paper
moderately moistened, and a trifle larger than the drawing, then a
blotter, a Bristol board, and a thick card, and draw through as before.
The coated copy paper sticks tight to the zinc after the first rolling;
it also retains the drawing in its first position, and allows repeated
rolling. If the original was over-moist when |75| copying, it sticks
to the zinc and separates with difficulty; if the moistening was just
right, two perfect copies can often be made from the same original.

I have attempted to copy drawings on a fatty zinc surface, and to etch
them strongly, but, far from being satisfied with the result, I prefer
the above method.

(_b_ and _c_) Copies of lithographs, type, plates for printing of any
kind, plates for _deep_ printing, I make on well satinized copying
paper*; in making the prints, I employ a copying ink as thick as
possible, with the addition of a few drops of a thick solution of
asphaltum in lavender oil, rolling a long time with but little color,
so as to get a sharp rather than a heavy print.

* Instead of the paste-gelatine-chalk, I prefer to prepare
the surface with a decoction of semina psyllii.

Plates for _deep_ printing, I heat equally throughout before applying
the color. Instead of color, I rub them with chemical Indian ink, wipe
the surface carefully, even polish it finally with a ball and some
Frankfort black. I then draw it through and again heat it uniformly, so
that the copy comes off of itself. Fine, sharp transfers, with perfect
relief, are thus obtained.

(_d_) Anastatic copies are no longer of great value, since they always
turn out roughly and cannot compare with photographic copies. Although
I possess a safe method, I believe that I will have to omit it on
account of the limited space of my work and the minute importance of
the results.

(_e_) Photographic fat or resin prints should be treated like ordinary
prints. Moisten them on the back with water—which is preferable to
placing them between moistened blotting-paper, since the drawing does
not grow too wet—and wait till they are easily flexible. Drops of water
on the film can and often do destroy the proof. Draw the plate through
with increasing pressure and one intermediate moistening. Prints in
fatty inks necessitate a temperature of plate of 35° C. Prints with
dissolved etching varnish (resin) as a printing film should have from
50°–60° C. When loosening the paper avoid warming, but moisten well.
Sticking of the gelatine film happens, especially with Husnik’s paper;
a safe remedy is to dry the copy in strong light, after developing.
Old sensitized paper, on the contrary, seldom sticks at all, and fresh
paper should always be sought.

In printing with the rolling press, I observe that the rollers of the
press need only once to be regulated, and that greater or less pressure
can be attained by thicker or thinner covering of the print with
sheets of paper. This gives much greater security than can be had when
constantly readjusting the rollers. |76|

THE FURTHER TREATMENT OF THE TRANSFER.

Should we now proceed directly to etch the copy, the acid would act
through the drawing, which is as yet but loosely attached to the zinc,
and would at last cause the lines to appear broken, if not destroy them.

It is, therefore, necessary to replace the loose copy by a possibly
dense etching varnish, attached fast to the zinc, and to produce an
intimate connection between the latter and the etching varnish. Here we
meet a difference between the French and Austrian methods. The former,
totally based on the lithographic process, favors the use of a resinous
dense color as a _strengthening material_, whereas the Austrian method
employs an ordinary copying color and endeavors to form an etching
varnish by sprinkling and melting in a quantity of finely pulverized
resin. In the method of etching with copper sulphate, it was attempted
to restrict the corroding action of the sulphuric acid by the following
method: The drawing, rubbed with color and thinly besprinkled with
resin, was slightly melted in, then sprinkled and rubbed with the
finest silver graphite or real water-gold. It was thus made an electric
conductor. A thin coating of copper was then deposited on the drawing,
which, in point of fact, hindered the destruction of the film. At the
same time, however, the process became uncontrollable, since often a
deposit of amorphous copper became tightly fastened to the metallic
surface. The lateral action could not well be ascertained, since the
narrowest parts were often clogged with metal, without preventing
corrosion from below.

The French method of etching is this: A thick solution of gum-arabic
is mixed with extract of nutgalls; this is carefully spread over the
surface of the plate by means of a fine sponge, and dried by a fan.
Then a knife’s point full of etching color (composed of 500 grammes
chalk color, 40 grammes coagulated mutton suet, 40 grammes soap, 125
grammes yellow wax, 40 grammes margarin, and 40 grammes oleine, melted
in the warm bath and passed through the color mill) is dissolved in
oil of turpentine, and a portion of this solution is spread uniformly
on the grinding stone by means of a fine sponge, so that the latter
contains a similar layer of color throughout. The fatty gum film
is then washed, with a wet sponge, free from fat and acid; a fresh
quantity of the gum and nutgall solution is poured out, and the copy
is by degrees strengthened by rubbing on the etching color with a
sponge. This is repeated until the drawing has attained the proper
strength throughout. The superposed layer of gum is then washed off,
the superfluous water is removed with a sponge, a wet cloth, and
blotting-paper, dried with a fan, then gently warmed. |77|

Now the plate is to be dusted with the finest pulverized resin,
consisting of equal parts of Syrian asphalt, washed in alcohol, and of
mastic; the superfluous resin is removed with a brush and some cotton;
the plate is then carefully heated, without beginning to melt the
resin, however.

This, by the French method, finishes the plate for etching. Only weak
acid is safe for such a plate, however.

According to the Austrian method (practised by me for several years),
we proceed as follows: The copied plate is first copiously coated with
a cold saturated solution of gallic acid, and then with a pure solution
of gum. Without allowing it to dry, I remove the superfluous preparing
materials with a wet sponge, and pour on some fresh gallic acid, as
with an excess of acid the drawing assumes a more brilliant black color.

The strengthening with ordinary copying color I effect, as the case may
be, with the rollers, the sponge, or by coating.

(_a_) _Strengthening with the Rollers._—I roll out some thick copying
ink with good, rough rollers which have been frequently used, and begin
to roll the transfer plate while still damp, without any pressure, till
its surface begins to dry. I then grasp the handles of the rollers
more firmly and blacken the dry plate uniformly, giving it a thin
coat of ink. This done, I moisten it a little and roll it regularly
with rollers freshly treated with color, so that the picture comes up
harmoniously and strongly.

Rolling off during drying keeps the gum solution from the drawing while
drying on, and keeps open the connection for rolling in.

Before going further I will explain the terms used*: To roll in is
to give color or ink, and is done slowly, with tightly grasped handles
and certain pressure. Rolling off is effected with loosely grasped
handles, without pressure, and quickly, and is intended to draw off
with the rollers any excess of color on the plate. _To work out_ or
_make the rollers_ means to bring fresh color on it from the grinding
stone, and is done with strong pressure and strong traction. The
correct management of the rollers rests in the wrists. To _reverse the
rollers_, to _change the handles_, means to turn the rollers around,
to make the left-hand handle the right-hand one, and thus to correct
irregularities in the distribution of color. After every advance and
return on the stone or plate to be blackened the rollers are newly
adjusted. The plate thus strengthened must be well |78| washed with
clear water, to be dried, and at times even to be retouched with a
brush and color dissolved in oil of turpentine.

* Color and ink are synonymous. “Burn in” and “melt in” mean
the same.

(_b_) _Blackening in_ with a sponge. The initiatory etching is done
with gallic acid, the gum coating put on and additional gallic
acid poured over; then some turpentine solution of copy color, the
consistency of syrup, is rubbed over the plate until the picture is
uniformly strengthened. If, as may happen in hand-drawings, the color
should become massed and not attach itself smoothly, it must be washed
off with turpentine and then clean color must be rubbed on.

This operation requires great delicacy. After having finished the
blackening in, rinse well, dry with a sponge and thick blotting paper.
Heat, so as to vaporize the last remnants of dampness, and retouch.

(_c_) A peculiar method of strengthening, nowhere described, as far as
I know, is that of drying the plate after coating it with gum, then
washing the gum with water; then, after drying, of covering the plate
with a thin solution of wax, asphaltum, rosin, and shellac in ether,
and of carefully coating the quickly drying film with gum. The film
remains on the lines of the copy, but easily detaches itself from the
bright metallic spaces, which have an insoluble combination with the
gallic acid and gum, and are thus protected from the fat.

_Faults in strengthening_ are caused by the following:

_a._ By ink which is too thick or too thin, or which has not been well
ground. Stripes are caused by the dissolving of the color which is
already present.

_b._ By excessive dampness on the plate (it does not take the color;
the color in the sponge changes to a slimy emulsion).

_c._ By too great pressure with the color sponge the fine parts are
lost. The same is the case with careless washing of the color of
hand-drawings.

_d._ In _rolling on_ excessive moisture on the plate spoils the work.
The surface of the rollers becomes glossy and must be again inked.

_e._ In pouring out the ink a very thick layer prevents the
strengthening of the finest lines.

Dirt on the plate often comes from handling the drawings; it must be
scratched off and the plate must be perfect before proceeding.

Now comes the changing of the ink into an etching varnish. But before
beginning we must cover the free edges of the zinc for the distance
of half a centimetre around the drawing with a solution of ink in
turpentine; the same applies to large white surfaces in the drawing,
which it is more convenient to cut out with a scroll saw. Then subject
the plate to the finest asphaltum |79| powder, passed through a
hair-sieve, and cover it by the dusting brush copiously with powdered
rosin. Continue the rubbing on of fresh powder for a minute, until the
ink is saturated, then dust out the superfluous powder with the dusting
brush and fine cotton, so that the metal is bright (no film should be
perceptible on looking over it).

The plate should now be heated to about 60° C., till the color of the
asphaltum changes from a coffee tint to a dead (matt) black. Place the
plate in this condition a second time with the asphaltum, which is
again absorbed rapidly. Dust off carefully as before and burn in again
till the color changes to a somewhat shiny black; the yellow tint must
be avoided, because this degree of burning exposes the lights in the
closest hatchings to the danger of running together.

Thus the coat of color is changed into an etching varnish of excellent
resistance and adhesion, and the plate is ready for etching.

THE ETCHING AND ITS INTERMEDIATE TREATMENT BEFORE MOUNTING THE CLICHÉ.

_Introductory remarks._—If we examine a wood cut or an electrotype with
regard to the depth of its narrow and wide-line complexes, we can at
once determine a plane for the closest hatchings; in a uniformly deep
layer the lines lie at a moderate distance apart, and those of the
highest lights are very deep. These three planes are situated higher
or lower according to the very narrow or very wide series of lines.
This gives a natural division of the different stages of etching, and,
according to the three depths, we distinguish the _sharp etching_ or
_etching on_ in which the engraving must advance far enough to place
the narrowest portions sufficiently low; _middle etching_, which has
to accomplish the same for the moderately narrow portions, and _deep
etching_, which must attain sufficient depth for the highest lights.

On account of the lateral action of the acid it is impossible to etch
down perpendicularly, but a wider covering is taken for each stage. Of
these wider coverings there remain after etching all around the relief
two terrace like grades, which must also be removed.

We have, then, in addition to the above, three sorts of etching, a
_round etching_, in which the grade remaining from the deep etching is
to be removed, and a _clean etching_, or a removal of the wire-edge
left after middle etching.

This natural subdivision is found in the old French method as well
as in the |80| new method, and both coating and the acids are of a
strength proportionate to the different stages of the work.

We have already alluded to the lateral action of the acid; it is a
factor that taxes the care of the etcher in the highest degree. In the
beginning of the action of the acid, the edge of the metal under the
coating is exposed the more, the longer the action lasts; here, of
course, the dissolving power becomes apparent. The deeper we go, the
more the metal under the line is exposed, and the action on the lateral
edge continually increases. In the effect of the acid we distinguish
thence, a perpendicular and a lateral action. Since the latter cannot
be removed by changing the character of the acid, we must give it a
part in this process of dissolving metals, but at the same time must
invent a method which will prevent the lines from growing thin.

But in order to do this we must know the relation of the perpendicular
to side action. Both are in proportion, a result both of theoretical
and practical consideration. In order then to attain a certain depth of
etching, a proportional lateral protection must take place, which is
by degrees destroyed by the lateral action. Since this lateral action
sets in at the beginning of the work, the dimension of the line must
be secured from the start. This is done in the Vienna method by the
already mentioned formation of the etching varnish, by means of dusting
with resin and burning in, by which an almost imperceptible growing of
the width of line is attained. The French method endeavors to correct
this by using a very weak acid and a correspondingly thin coating,
but coating oftener and etching at every new coating, as we shall see
below. Also the coating for middle and deep etching must be arranged in
accordance with the principles above elucidated. As deep as the middle
or deep etching is desired, so wide must the lines be surrounded by
etching varnish.

ETCHING BY THE FRENCH METHOD.

We have already seen (p. 76) how a copy is made by the French method
for etching, and we now continue the development of this process.

Into a tray pour 4 litres of water at 18° C., add 15 c.cm. nitric
acid and mix well by shaking. Then place the prepared plate into the
bath and rock it for seven or ten minutes (according to the fineness
of the drawing), rinse well with water, remove the remaining water
with blotting paper, and, finally, dry thoroughly with a fan. (Do not
forget to dry the back.) Now warm the plate from the back, moving the
flame about continually, so as to secure uniform heating and prevent
warping of the zinc. The asphalt powder, which is as |81| yet but
loosely attached, is more intimately connected with the subjacent ink
through this heating process. The combination becomes evident from
the assumption of a black lustre. With the appearance of this, stop
heating, and lay the plate on a cold stone to cool. This done, spread
some gallic acid over it with a soft sponge, and without washing it
off, spread gum on the surface of the plate, and hasten the drying with
a fan.

Mix some etching ink with varnish and work it out into a thin layer
with good rough rollers. If the rollers are in order, wash the coat of
gallic acid and gum from the plate, remove superfluous water and _roll
in_ (the manner similar to that used in lithography). The surface of
the plate should not be more than moderately damp, so that the rollers
may not slip. If a coat of color has been uniformly deposited, wash the
plate with clean water, remove the excess with a sponge and blotter,
dry by fan and remove all moisture by heating to 45° C. Dust the warm
plate again with asphaltum (remove the excess), and warm it a trifle
to secure better adherence. Strengthen the bath by the addition of
15 c.cm. nitric acid, and etch again for seven or ten minutes under
continued shaking. Then rinse the plate, remove the water and dry with
a fan, and burn in the resin powder well. Careful inspection will now
show a successful and uniform but still weak relief.

As before, the plate is coated with gallic acid and solution of gum,
is dried, washed, and _blackened in_, in which treatment one-third
“wax pomatum”* is mixed with the etching ink. After washing and
drying heat the plate up to 60° C., thus causing an imperceptible
widening of the drawing. After coating dust once more with asphaltum,
warm it and cover only the back and the white rim around the drawing
with a solution of shellac (1 part ruby shellac in 10 parts spirits).
Strengthen the bath with 20 c.cm. of acid and bathe it for seven to
ten minutes, shaking the bath regularly. Continue until you see that
the lateral action of the acid has almost wholly destroyed the lateral
covering produced by heating. Do not, however, etch too long, and do
not mistake the _over_-hanging coat for the other. Then follow washing,
drying, melting on some resin, cooling, coating with gum, blacking
in with equal parts of etching ink and “wax pomatum,” then washing,
drying, greater heating (70° C.) (so that by increasing the ink each
line receives lateral protection), cool and dust to excess with the
finest resin dust. |82|

* Wax pomatum is prepared by cutting beeswax into fine
parts and covering it in a wide-necked flask with oil of
turpentine. In a few days a jelly-like mixture will remain,
which serves the above purpose.

As we have now reached the necessary depth for the narrowest portions,
we use, instead of the asphaltum, resin, which melts easily and spreads
out readily, in order to attain protection for our middle etching.

Strengthen the bath with 30 c.cm. acid, and bathe until the lateral
action of the acid has reduced the lateral coating to a narrow edge.
Then wash, dry, melt on some resin, cool, prepare with gum. Blacken in
as before, but employ one-third etching ink and two-thirds wax pomade
and apply so thickly that all the narrowest spaces of the drawing are
completely filled with color. Continue warming until the ink, which was
applied, has well covered each line; then dry and use resin as before.

The acid may now be strengthened by 100–158 c.cm., according to the
strength of coating chosen. Bathing must be continued until the edge
that has run off begins to grow narrow. Wash, dry, burn in resin, cool,
coat with gum, and blacken in by rollers with clean wax. Continue
heating until each line is well covered by ink. Always dust until the
ink is fully saturated and then heat gently.

Strengthen the bath 200 c.cm. and begin the _deep etching_. According
to the depth to be attained repeat the manipulation of strengthening
once or twice. Whenever a corrosion of the lateral coating becomes
apparent, coat freshly, adhering to the above order of operation. For
obtaining the necessary depth ink is applied about _ten_ times, adding
wax each time to facilitate the spreading when warming.

In order to attain a fine, regular lateral coating, great ability in
manipulating the rollers is necessary, since without such the correct
degree of strengthening is never attained. Irregular coating leads,
of course, to irregular melting of the ink; one spot then is already
sufficiently wide, while another is not yet covered. In such cases
coating with a brush must be resorted to.

If the necessary depth is attained, the plate is to be freed carefully
from the coating with a brush and oil of turpentine, and then placed in
fresh sawdust, which absorbs the oil of turpentine and leaves behind
a clean surface. Now the work can be criticised in all its parts. To
every coating is a corresponding narrow edge of etching, which is now
to be removed in order to make the plate fit for printing. To removing
these edges we must devote our attention. We begin with the top one,
and make preparations thus: Roll out on a clean, warm stone with
faultlessly smooth rollers a very thin gauze-like layer of etching ink.
Likewise warm the zinc plate and roll it in all directions without
pressure till the picture becomes beautifully black. |83|

Pressure must not be employed, but the coating must be obtained by
renewed _working out_ of the rollers on the _color-slab_, and repeated
coating. When at last the desired strength is obtained, dust with the
finest asphaltum powder, blow the traces of dust out of the hollows,
and warm till the layer becomes slightly brilliant. Next, etch in a new
bath of 4000 c.cm. of water and 40 c.cm. of acid for 7 minutes, wash,
and dry well; then, with more ink on the rollers, coat the dried plate,
dust once with resin, heat gently, then apply the asphaltum and burn in
strongly. Thus the first relief is protected laterally, and the first
grade can be etched down completely, without endangering the drawing.
To remove the second grade, we repeat washing, and put on etching ink
mixed with one-third wax. Rolling must continue till the narrowest
spaces of the etching are completely closed. Then follow dusting with
resin, warming, and placing the warm plate in the asphalt, dusting,
removing the excess, and finally burning in.

With this coating a further rounding of the grades can take place (in
a bath of 10° Baumé). Continue this process until all the grades are
removed and the etching appears as perfect as a cast plate.

Since hitherto all publications on chemigraphy have duly described
this method, I believe that I should not enter into further details,
improvements, etc. Suffice it to call attention to weak points. In
view of the new method later to be described, the reader may make a
comparison between the two.

A very weak point is the method of strengthening based on the
lithographic process of superimposing new color upon the old color.
In consequence of the repeated melting in of resin, this latter
acquires an uneven surface, which can be blackened in only with great
difficulty. Equally untrustworthy is the lateral protection by _melting
off_, which is only attained with safe uniformity by skilled workers.
And what is more, with the weak coating at the beginning; even weak
acid often works its way through to the etching, so that the finished
etching appears slightly porous, and gives no dense black print. Also
shaking, which is to promote the removal of the metallic mud and the
gas bubbles from the lines of the etching, has an unsatisfactory
effect, inasmuch as the single lines are often thus under-washed.

But the principal defect is that no accurate determination of the
degree of each operation can be made, everything depending on the
delicate execution of the process.

The time that the etching of a correct, deep cliché requires by this
method is from eight to ten hours. This procedure also demands better
trained hands |84| than the Austrian, which, in large establishments,
is based on a division of labor, and in which men trained in a single
manipulation, under good supervision, accomplish the maximum work
surely and excellently.

Furthermore, the expenses of the manufacture on a large scale are
far greater, since each etcher draws a greater salary than a workman
skilled in a few manipulations, such as the following method requires.

THE AUSTRIAN METHOD—THE ETCHING ON.

I have already shown how a transferred plate should be prepared for
etching by this method. Before proceeding to the details, however,
we will prepare the etching baths, which, by the way, may always be
employed for several plates. Corresponding to the three steps of
etching, we require three baths of different concentration to be
determined by means of an areometer with a Baumé scale. The bath for
_etching on_ is prepared in strength of 2° Baumé at a temperature
of 18° C. There must be a quantity sufficient to cover the plate to
a depth of 4 to 5 centimetres. The bath for middle etching requires
10° Baumé and a temperature of 18° C.; the bath for deep etching,
18° Baumé. These baths are prepared at the beginning, and are used
for the five successive stages of etching. If, after continued use,
the bath for deep etching should grow weak, it may be used for middle
etching. For protecting the trays, I recommend a coat of gutta-percha
over a well-coated inner surface of asphaltum. Everything being ready,
immerse the prepared plate in the bath, and with an etching-brush brush
the surface of the plate uniformly for two minutes.

The hairs of the brush must only rest lightly on the metallic surface.
For determining time, use sand-glasses of two, three, and five minutes.
After two minutes, take the plate out of the acid, wash it well with
water, and examine it carefully. If the effect has not been uniform,
see that two minutes more can be safely given in the etching bath. If
by any sort of careless handling the plate has been injured, dry it
with blotting-paper, vaporize the remaining dampness, and cover the
soiled spot with very thick solution of asphaltum in turpentine. Cool,
and continue brushing lightly for two minutes in the bath.

At the end of this time, wash and examine again. Even now everything
will be intact. With very fine drawings, however, lateral action has
already progressed so far that, under all circumstances, the exposed
edges must be covered. Coarser drawings generally stand one or two
minutes more.

To try the depth of etching: with your finger-nail on the edge of the
black |85| rim, feel how far the etching-on has proceeded. As soon as
the finger-nail catches, the depth is sufficient, and the sides of the
lines may be covered.

For this operation the plate needs, above all, thorough washing, drying
on both sides by blotting-paper and gentle heat, and a temperature
of 45° C. At this temperature place the plate into the finest
resin-powder, and rub the latter several times over the warm drawing,
using for this purpose a fine brush. The protection, which has grown
sticky through heating, retains a thin coating of resin, which, after
dusting off the bright metallic spots with a brush and fine cotton,
and after careful fanning off, is reheated to about 50° C. At this
temperature the plate is returned to the white rosin, receives a good
dusting-in, and being freed from excess as before, is heated to about
65°, so that the easily fusible rosin begins to spread out. At this
moment extinguish the light, and put the plate into the asphaltum,
which will attach itself copiously to the sticky resin. Brush the plate
well with the substance, remove any excess from the bright spots, heat
to 80° C.; then place it again into the asphaltum, brush it, clean
it by removing any excess, and heat it to 100° C., when a complete
combination of the resinous mass takes place, and a uniform etching
varnish is formed. This last coating is extremely regular, and it is
wonderful to see the accuracy with which the lines have been covered.
Beginners are warned to pay attention to the careful cleaning of the
bright parts of the plate when brushing and dusting it; should any
resin remain behind, it melts on, and grows by degrees to a strong
yellow tint, which is very difficult to remove, but very easy to guard
against. Never forget to dust off the back.

While the plate is still hot, lean it against the wall, face in, and
the back covered with a solution of shellac.

Now the plate is ready for further etching, which is carried on for two
minutes in the first bath. At the end of two minutes, wash and examine
critically. In almost every case we may etch for a third, or even a
fourth time. It is, however, sufficient for the beginner to know that
he has sufficiently etched in two spaces of two minutes each, after
preparing with resin. Trying and examining with the finger-nail on the
black edge will show a fine relief. Should it be possible to etch for
a third space of two minutes, or even of one, without danger, it is
preferable to do so. It should be a rule to proceed as far as possible,
judging from the character of drawing and coating. Experience is easily
gained in two or three trials, since anything can be examined at any
moment. Beginners would do well to use a magnifying-glass with good
field of view in examining, when they can observe the most sensitive
portion, and |86| all changes may easily be noticed. The brush should
be used lightly, to prevent scratching. Usually, it is fastened at
right angles to a stick to protect the hands from the effect of the
acid.

To raise the plates out of the tray, lay a gutta-percha thread into the
bottom of each tray, fastened at one end to the top edge of the tray,
projecting over the same on the other side. The plate is placed on the
thread while etching. It may be removed without touching the bath by
pulling the free end of the thread.

As already remarked, the spreading of ink on a surface which is more
or less rough is difficult. For this reason the plate, when etched-on
after my method, is to be washed out with oil of turpentine. A strong
brush should be used for this, and some of the oil rubbed over the
plate without pressure. You must cause a dissolving, not a rubbing off,
of the coat. On continuing the addition of turpentine, the metal grows
bright. Take, then, a handful of the coarsest of pine-wood sawdust and
rub off the surface. This removes instantly every trace of turpentine,
leaving a clean surface behind. For the sake of security, pour on more
turpentine, rub with a somewhat softer brush, and remove again with
clean sawdust.

It is important that the wash-table should always remain free from
sawdust, which latter should fall through the grating into a suitable
receptacle. If this rule is disregarded, the wash-brush will soon be a
conglomerate of sawdust and hairs. Sawdust and turpentine will stick to
the brush so tightly that a new brush will have to be purchased.

Now we again examine our work. It is a mark of success if the relief
still shows its original smoothness in all its parts, and has nowhere
grown porous. All the parts must be clear in their correct proportional
strength, as seen in the transfer.

The treatment of the plate from the time of transfer to the close
of the etching-on takes: for the saving of the edges and the white
portions of the drawing, 2 minutes; for preparing twice with asphaltum,
4 minutes; for varnishing the back and coloring the plate, 4 minutes;
for etching-on the lateral protection, 4 to 5 minutes; for preparing
twice with resin, asphaltum, and varnishing, 16 minutes; for renewed
etching, 4 to 5 minutes; and for washing, 5 minutes—that is, 33 minutes
in all. Add 7 minutes for inspection and retouching, and 40 minutes
will be the space allowed for etching-on. |87|

MIDDLE ETCHING.

In order to give to the middle tints of the drawing the depth necessary
for printing, we begin with a new blacking-in. We need for this purpose
excellent, smooth, and hard rollers, which are immersed in minium and
linseed oil, and are then left to dry for a short time. Contrary to the
French method, we need here a thin composition for the etching ink,
obtained by concocting equal parts of paraffine, suet, beeswax, and
ordinary ink, prepared in an excess of good linseed oil. (Ready-made
color of right composition may be had of E. Liesegang, in Dusseldorf,
and other dealers.)

This color, when of right composition, possesses the power of absorbing
resin-powder, and changes in combination with the same, when heated, to
a compact, very solid, yet brittle mass.

Of this color, which is soft as butter, take a portion on a
knife-point, and spread it upon the smooth rollers, forming a perfectly
uniform layer. The complete covering is done by rolling, changing the
adjustment at intervals. When a perfectly uniform, oily coat is spread
on the color-slab and the rollers, begin rolling-in the washed plate.

Do not exert any pressure, but roll, carrying the handles so as to
black the relief only from the surface of the rollers. Of course,
it cannot be prevented, and is of no consequence, if ink attaches
itself to the large white spots. Rolling continues till the oily brown
coating has deposited itself uniformly. Exercise care in order not to
get more ink on some spots than on others. The plate, now completely
rolled, is placed in the finely powdered resin, with which it must
be completely covered. For the space of two minutes the oily color
absorbs the powder, which should, therefore, be strewn on it and rubbed
off repeatedly. If saturation in the cold has taken place, dust off
lightly with brush and cotton, blow off well, and heat uniformly to
35° C. The resin should not melt now, but should only grow sticky and
combine intimately with the color, which forms the binding material.
This change is observed immediately in the change resulting in the gray
resin coat. As soon as the change occurs (beware of unequal heating),
again place the warm plate into the resin, saturate as before, dust
out, blow strongly on the bright, metallic spaces, to remove remaining
traces of resin, and heat to 50°–55° C. At this temperature cover the
film with fine asphalt powder, dust off as before, and heat to 65° or
70° C. In this condition the plate is again saturated with asphalt,
and the layer, after careful dusting and blowing, is heated until it
grows slightly |88| brilliant. Thus a complete coating is formed, and
the plate has the appearance of Fig. 6. The black spots represent the
dirt which has clung to the intensest lights, and must be removed.
But before attempting this, we varnish the back of our plate with a
solution of shellac, and cool it completely in water.

[Illustration: Fig. 6.]

Now take a very coarse scraper, ground with a sharp edge; hold it
between the index and middle fingers, and scratch away the dirt from
the light spots, making the edge of the scratcher draw the strokes
close together. The brittle backing breaks off finely, and in a few
minutes the dirt is removed and the plate is ready for etching. If
(which will only happen to beginners) the drawing should be scratched,
the exposed spot must be covered, by means of a brush, with a thick,
warm solution of asphalt in turpentine; the dirt which was scratched
loose is brushed off, and the plate goes into the bath for middle
etching for about three minutes. Brushing and washing follow in the
same way as in the previous operation. At the expiration of three
minutes inspect (with or without a magnifying glass); places that have
been uncovered must instantly be covered with asphaltum, as already
directed. Etching is continued till the lateral coating no longer
protects the first relief, which generally takes place after the third
period (in about nine minutes) in a new bath, but requires twelve
to fifteen minutes in an old one. It is proved by the existence of
only a narrow thread alongside of the relief. The moment can be well
ascertained. If we wish to be sure of it we may do so by exposing the
edge of the black rim at different places; the width of the thread
is then apparent, and a safe conclusion may be drawn from the single
spots as to the whole plate. If not enough middle etching has taken
place, the thread remains wide and requires an extraordinary clean
etching, which may lead to the picture growing thin and endanger the
finest lines. Care, then, is necessary to ascertain the right moment of
suspending the middle etching, and of continuing in the above-described
manner with oil of turpentine, brushing, sawdusting, and washin…

source: Project Gutenberglicence: Public domain (per item)year: —id: 52378citation: https://www.gutenberg.org/ebooks/52378characters: 200,001

record · JSON · record JSON

Related services and records

Services

  • Estate — measured countries, lanes and facts
  • Intel — live corroborated events
  • Legal — statutes, cases and citations
  • Encyclopedia — articles with inline sources
  • Space — launches, satellites and orbits
  • Search — federated search and reports
  • Pass — passport account and SSO
  • Corpora — read-only corpus origins
  • e01 — self-hosted corpora and tools

Text and metadata only; each target carries its own sources. Missing data is published as no-data, never estimated.